50 sand
20 1/4 soda ash
9 1/16 hydrated lime type N
5 1/4 Potassium carb
3 3/16th Borax 5 mole


I'd like to be clear on this because I'm taking notes and rubbing my hands together in planning for the future. Muahahah.

While we're at it ...

Quote:
Originally posted by Pete VanderLaan
The first formula does have a ton of silica and it is durable and the silica content is why the glass works well in a torch. It was a glass I used that I cut and polished a lot and it polishes beautifully. That is because of the potash.
Is that in reference to this:

100 Sand
28 Soda Ash
14 Lime Hydrate
12 Potassium Carbonate
200 grams potassium nitrate
100 grams antimony oxide


And finally ...

Quote:
Originally posted by Pete VanderLaan
The second formula is a glass designed to fit SP87 hand in glove. I use it for my red and opal silver amber formulations when matching SP87. It also makes a very nice turquoise blue I am currently working.
Is that in reference to this:

63.25 silica
20.25 soda ash
9.06 Hydrated lime type N
2.18 Borax 5 mole
5.25 Potassium carb
100 grams antimony oxide
130 grams potassium nitrate