David:

I have been melting SP87 for 3 years now in my Denver 135 # furnace.

When I charge, I usually let the furnace sit at whatever the working temp. was until I put the last of the batch in to fill the crucible. Then I ramp up to 2225 and let it cook for 10 hours, drop the temp. to 1900, let it squeeze for 2 hours then ramp up to 2050 where I work at.

I almost every time come out with beautiful clear, bubble free glass.

I am going to try Gaffer in the fall and see what happens.

Good luck,
Ed