Additionally there is from Zicar
MICROSIL Microporous Insulation
Max Use Temp 1742F
68F .132
392F .145
752F .173
1112F .208
1472F .263
Alumina Mat
Max Use Temp 3002F
315F .50
1000F .77
1400F 1.03
1796F 1.33
2192F 1.65
2597F 2.15
Alumina Blanket Type AB & MB
Max Use Temp 2912F
599F .50
1000F .70
1400F .90
1796F 1.25
2192F 1.60
2597F 2.15
Alumina-Silica Blanket Type ASB-2300 & ASB-2600
Max Use Temp 2300F and 2600F
Bulk Density of 4 pcf
500F .56
1000F 1.13
1500F 1.96
Bulk Density of 6 pcf
500F .45
1000F .94
1500F 1.70
2000F 2.80
Bulk Density of 8 pcf
500F .39
1000F .78
1500F 1.31
2000F 2.02
Bulk Density of 10 pcf
1000F .73
1500F 1.17
2000F 1.72
Alumina Insulation Type ZAL-15 & ZAL-15AA board
Max Continuous use 2822F & 2732F
482F .40
977F .60
1472F .90
1967F 1.30
2282F 1.70
2462F 1.80
Alumina-Silica Insulation Type AXL Board
Max Continous Use 2300F
752F .80
1472F 1.20
2012F 1.50
Alumina-Silica Insulation Type AXHTM Board
Max Continous Use 2600F
752F .60
1472F 1.00
2012F 1.70
There are a few more if anyone is interested.