Lino's Nero Tea

That's what we called it at Manifesto anyway.

Sand 100
Soda 44
Calcium 16
Boric Acid 3
Sulphur 3.950
Rosin 1.3
Iron Oxide 2.850
Black Nickle Oxide 1

Just for cane or threading. Overlay onto gaffer duro white for extra opaqueness in those super stretched out cane pick ups. Fun to melt. Not as bad as Pete would have you believe

Have fun kids.