zinc oxide

Going to try a recipe from the forum (Mr. Vanderlaan) which calls for zinc oxide, as follow:

"I have made calcedonia's in cullet in the past but it is difficult in a cullet that is oxidizing in nature. In about eight pounds of actual glass, I would recommend adding 4.6 grams of silver nitrate, 28 grams of zinc oxide and 28 grams of black tin. Then add two grams of red iron which is key to success in this glass. The iron allows for nucleation points in the glass ( places where crystals or colloids like to form). Melt the glass kind of cold- about 2180F. Melt in a neutral environment. When you gather it, allow the gather to really cool down and then reheat it hard in the gloryhole. If it is going to strike, that will make it happen. Repeated heats intensify the color."

US pigments has a normal zinc oxide and a calcinated one. Which would work better in making color?
Reply With Quote
  #2  
Old 07-07-2017, 02:19 PM
Greg Vriethoff's Avatar
Greg Vriethoff Greg Vriethoff is offline
(((0)))
 
Join Date: Jan 2007
Location: Charlotte, NC
Posts: 1,900
Greg Vriethoff is on a distinguished road
I couldn't resist

Not helpful, I know.

https://youtu.be/lLp4DZmPqYE
__________________
"It's such a fine line between stupid and clever." - David St. Hubbins
Reply With Quote
  #3  
Old 07-07-2017, 02:43 PM
Dan Vanantwerp Dan Vanantwerp is online now
Registered User
 
Join Date: Apr 2017
Location: Bozeman, MT
Posts: 154
Dan Vanantwerp is on a distinguished road
...and no calcedony glass either!

Perfect!
Reply With Quote
  #4  
Old 07-07-2017, 03:22 PM
Josh Bernbaum Josh Bernbaum is offline
Registered User
 
Join Date: Feb 2009
Location: Brattleboro, VT
Posts: 533
Josh Bernbaum is on a distinguished road
I've just used their (US Pigment) regular ol' zinc oxide for some of my melts, but that was for certain transparent bases. I haven't done any chalcedony but it's so little in the formula you quote here and he says zinc oxide so I'd go with that.
__________________
www.jmbglass.com
instagram.com/joshbernbaum_glass
Reply With Quote
  #5  
Old 07-07-2017, 04:48 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 19,825
Pete VanderLaan is on a distinguished road
The zinc is represented as an opacifier. try it at the least. The black tn is at least equally important. My formulations come from a batch glass, not a cullet but in the earlier years it worked well based in a plate glass cullet which is rich in iron. I'd be inclined to melt low (2200F) or less. It needs the iron, tiny as the amount is.

It may not work of course. There's no guarantees..You have to expect failure and to keep up your search. If it was easy, every one would be doing it.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #6  
Old 07-08-2017, 12:14 AM
David Hopman David Hopman is online now
Registered User
 
Join Date: Mar 2009
Location: Sutter Creek, CA
Posts: 414
David Hopman is on a distinguished road
Quote:
Originally Posted by Greg Vriethoff View Post
Not helpful, I know.

https://youtu.be/lLp4DZmPqYE
That's exactly what I was going to post.
Reply With Quote
  #7  
Old 07-08-2017, 09:15 PM
Rich Samuel's Avatar
Rich Samuel Rich Samuel is online now
Registered User
 
Join Date: Apr 2002
Location: Seattle, WA
Posts: 2,300
Rich Samuel is on a distinguished road
They should restore it and do a 40th. anniversary re-release. Most of it still cracks me up.
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is Off
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 03:42 PM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2018, Jelsoft Enterprises Ltd.
CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.