Erbium Pink, Brossphate Opal

I've been goofing around with Dave's awesome opaline recipe and an erbium recipe I cooked up. The phosphate opal at 2.6% doesn't do much out of the pot for me in my process which is thin cups and some glassybaby tests. It does, however, make an excellent, beautiful, consistent, striking fire opal in bar form, which I've shown here. I plan on doubling the phosphorus on the next melt and see how it goes for me.

I also melted a 10% transparent erbium. I made an educated guess on how low the erbium would take the expansion and my initial adjustment, before melting, turned out compatible. I'm going to try and lower it 1 point to get it spot on but I was pretty thrilled with that. This stuff is expensive. One less melt to pay for. Erbium also does a color shift from "it's a girl" pink in daylight or incandescent light to a pretty electric fuschia under florescent lighting.

So what I have here is Dave's opal turned into bar and then overlayed and then the same thing but with a hot dip of the erbium pink. I just love the juicy transparent layer on the bottom of this piece.

I'm also loving that this forum is on to page two already. Thanks Pete for breaking this one out. It's pretty convenient to be able to see it all in one place.
Attached Images
File Type: jpg Bross opal resize.jpg (74.8 KB, 65 views)
File Type: jpg Erbium resize.jpg (87.2 KB, 70 views)
__________________
WWUD? Think for yourself.
Reply With Quote
  #2  
Old 01-12-2018, 06:11 PM
Dan Vanantwerp
Guest
 
Posts: n/a
Looking very good! Brossphate...classic.

I asked if he wanted a royalty if it was mixed by a batch company (which he didn't). Wonder if he'll change his mind with a brand name like that just waiting to be had.

I've had no luck getting this or Pete's base mixed by Spruce Pine or East Bay. Might try Jim again now that the holidays are past. I've priced everything through Seattle Pottery and will get my own small stock of batch ingredients soon. Hope I can catch up to you and share some experiences. Controller went out on my furnace so I'm cold for a couple weeks.

Hmmm...2 pages of threads with hundreds of posts starts to sound like a book, doesn't it?
Reply With Quote
  #3  
Old 01-12-2018, 06:55 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,506
Pete VanderLaan is on a distinguished road
I got almost the identical color in a strontium phosphate based solely on Dave's using selenium which is a lot cheaper. Getting the calcium out of that glass certainly is a key. Keeping the potassium high works as well in the stuff of Dave's as it does in any traditional high potash/ selenium glass body.

There's some very big changes ( as in tectonic) coming very soon in the retail color industry.
I may consider mixing my clear in small quantities and selling it. that's different than the changes I refer to.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #4  
Old 01-12-2018, 11:34 PM
Eben Horton Eben Horton is online now
Registered User
 
Join Date: Apr 2002
Location: Wakefield, RI
Posts: 4,573
Eben Horton is on a distinguished road
Quote:
Originally Posted by Pete VanderLaan View Post
I got almost the identical color in a strontium phosphate based solely on Dave's using selenium which is a lot cheaper. Getting the calcium out of that glass certainly is a key. Keeping the potassium high works as well in the stuff of Dave's as it does in any traditional high potash/ selenium glass body.

There's some very big changes ( as in tectonic) coming very soon in the retail color industry.
I may consider mixing my clear in small quantities and selling it. that's different than the changes I refer to.
What changes are you talking About? I have a hunch as to what it is... someone is going to retire?
__________________
<eben epoiese>
Reply With Quote
  #5  
Old 01-13-2018, 09:18 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,506
Pete VanderLaan is on a distinguished road
I really can't, not because I'm hiding stuff ( I am ) but because I don't know critical details that I'm dying to know. It is still possible for it to not happen to the extent it currently is resolving. I think it will go public in the next few weeks. I view it as huge.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #6  
Old 01-13-2018, 11:10 AM
Eben Horton Eben Horton is online now
Registered User
 
Join Date: Apr 2002
Location: Wakefield, RI
Posts: 4,573
Eben Horton is on a distinguished road
Quote:
Originally Posted by Pete VanderLaan View Post
I really can't, not because I'm hiding stuff ( I am ) but because I don't know critical details that I'm dying to know. It is still possible for it to not happen to the extent it currently is resolving. I think it will go public in the next few weeks. I view it as huge.
Ok. Well... is it good news or bad news ?
__________________
<eben epoiese>
Reply With Quote
  #7  
Old 01-13-2018, 11:10 AM
Eric Trulson Eric Trulson is online now
Young Turk
 
Join Date: Sep 2014
Location: Boston
Posts: 115
Eric Trulson is on a distinguished road
Thanks for sharing and being specific about your process Jordan, both those colors look great.

Especially nice to be able to compare the same shape with just the opaline and then with a gather of transparent over it.
Reply With Quote
  #8  
Old 01-13-2018, 04:54 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,506
Pete VanderLaan is on a distinguished road
Quote:
Originally Posted by Eben Horton View Post
Ok. Well... is it good news or bad news ?
**
Well, I hope it's good. It could be. It will be different.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #9  
Old 01-14-2018, 09:41 AM
Victor Chiarizia Victor Chiarizia is offline
Registered User
 
Join Date: Sep 2005
Location: fairview, NC
Posts: 560
Victor Chiarizia is on a distinguished road
ok thanks pete. you let my cat out of the bag.
so yes i'm buying gaffer color and sp batch company. what else do i do with a lottery winning? and i'm raising the price of everything too. v
Reply With Quote
  #10  
Old 01-14-2018, 09:54 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,506
Pete VanderLaan is on a distinguished road
Quote:
Originally Posted by Victor Chiarizia View Post
what else do i do with a lottery winning?
*********
I didn't mean to expose your good fortune. I think buying Spruce Pine is a good move. Get it with Erbium. It can serve as a sandbag operation in a pinch when Nuclear war comes to the Smoky Mts. You already have the gun.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #11  
Old 01-14-2018, 10:45 AM
Dave Bross Dave Bross is offline
Registered User
 
Join Date: Apr 2002
Location: Archer FL(near Gainesville)
Posts: 2,954
Dave Bross is on a distinguished road
Getting back to the glass color....

The percentage in the phosphate Jordan mentions requires multiple strikes (hot-cold-hot-cold) to get dense opaqueness. I first figured it out making furnace beads and that process had a number of strikes as a default. It can be made quite opaque with three or more strikes.

Coming out of the pot clear has other advantages. You can make multi layer transparent/opaque veils by repeat gathers with no reheats (not striking it any further).
I never got to it but I wanted to see what the minimum percentage of phosphate would be to just barely strike. I thought that would open up other avenues. Something like the old Fenton stuff that only struck when it touched the mold.

I have some distant memory that there is a ceiling on how much phosphate you can add. If you dig back in classics to the original post you'll find the link to the original Corning patent that tipped me off on this. I think it mentions a max on phosphate.

I'm laughing at the Brossphate name tag. Could this be my 15 minutes of fame?

No royalties required. I'm just an open source kind of guy. I never would have figured that out without all the other info that everyone posted here over the years prior to that.

As Pete says, potassium content in this glass does good things.

The phosphate is slightly dichroic too. If I'm remembering correctly, it's red for transmitted light, blue for reflected.
__________________
Art is not a thing...it's a way.
Reply With Quote
  #12  
Old 01-14-2018, 05:34 PM
Jordan Kube Jordan Kube is offline
?
 
Join Date: Aug 2003
Location: Seattle, WA
Posts: 1,698
Jordan Kube is on a distinguished road
It's a really nice glass, Dave. Thank you. I've been wanting to melt it ever since you got it figured out years ago. I've been reading through all those old posts and I think the max is like 5.5 - 6%.
__________________
WWUD? Think for yourself.
Reply With Quote
  #13  
Old 01-14-2018, 07:48 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,506
Pete VanderLaan is on a distinguished road
Robert Held NECCA confernence 1968 ( pre GAS) . At that presentation Robert Asserted you could Add Up to 5% Phosphate using bone ash 21 ( don't even try) to the base clear BATCH glass without experiencing issues on mismatch.
Attribution:

That' s Robert Held, so you're clear. ( Alive and involved)

I tried it and it worked. The Strontium is indeed a big step ahead, Thanks Dave, Thanks Milos (R.I.P.) . It works too. Fire opals by their vary nature always have the blue / red transmission characteristics.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #14  
Old 01-15-2018, 11:20 AM
Dave Bross Dave Bross is offline
Registered User
 
Join Date: Apr 2002
Location: Archer FL(near Gainesville)
Posts: 2,954
Dave Bross is on a distinguished road
I'm thinking the strontium has application in transparent glasses too. Volf mentions that it was being used to replace up to half the lead content for TV tube glasses. If I'm remembering correctly, without digging out Volf and comparing numbers, it gives it a greater modulus of elasticity like lead. Not to mention it's probably makes for a more clean "crystal" appearance for transparents.
__________________
Art is not a thing...it's a way.
Reply With Quote
  #15  
Old 01-15-2018, 11:43 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,506
Pete VanderLaan is on a distinguished road
Mark told me during the color classes that he had only used strontium in his glasses for the last 20 years with the exception of calcium monophosphate which is quite hard to find these days. He, like many , consider calcium to be a really trashy material. My glasses don't have much calcium if any these days. I do use Barium and zinc much more. If I have calcium, it's always in a 1/3 ratio with barium. I tend to use Sodium tri phosphate as opposed to tri sodium phosphate. I'm not much of a fan of sodium either.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #16  
Old 01-15-2018, 06:26 PM
Scott Novota's Avatar
Scott Novota Scott Novota is offline
AbbyNormal User
 
Join Date: Jan 2004
Location: Pensacola Florida
Posts: 2,146
Scott Novota is on a distinguished road
Jordan,


Did you just cook that up in your little guy or did you make a big batch?
Reply With Quote
  #17  
Old 01-16-2018, 04:30 PM
Jordan Kube Jordan Kube is offline
?
 
Join Date: Aug 2003
Location: Seattle, WA
Posts: 1,698
Jordan Kube is on a distinguished road
The furnace holds a 38 pound crucible.
__________________
WWUD? Think for yourself.
Reply With Quote
  #18  
Old 01-16-2018, 06:13 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,506
Pete VanderLaan is on a distinguished road
I candled the baby furnace today: 2 13lb pots, one 80 lb pot.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #19  
Old 01-17-2018, 02:16 PM
Dan Vanantwerp
Guest
 
Posts: n/a
Whatcha gonna make?

Sounds almost exactly like my setup
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 11:23 AM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2019, Jelsoft Enterprises Ltd.
© CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.