Telux cullet

Does anyone have experience with cullet from Telux in Germany?
Iíve been using it in my wire melter in the UK. Bought it from Glassworks Services as White Water Nuggets (pucks about 2Ē diameter). Itís been good, apart from the popping during melting, even though I preheat. My problem is lack of experience as Iím learning so I donít know if I would find Cristalica easier. Too easy to blame the glass!
The composition is given on the Glassworks Services site as
SiO2 73.12% Al2O3 0.762% Fe2O3 0.007% CaO 7.420% MgO 0.142%
BaO 1.592% ZnO 1.605% K2O 4.607% Na2O 9.932% Li2O 0.674%
SnO2 0.006% Sb2O3 0.105% SO3 0.013% TiO2 0.012%
Reply With Quote
  #2  
Old 04-27-2019, 01:39 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,251
Pete VanderLaan is on a distinguished road
At that size, preheat the little slugs.
I've not heard of the cullet but cullet is undergoing a balkanization right now.
Test some small samples against the color you use
.
Googling it, I can only come up with Telus cullet, so you may have to put up more complete info. Glassworks services lists itself as supplying Kugler which is now making clear cullet that, as you say, explodes in the pot. Perhaps it's the same material but their website doesn't mention it.

It's quite high in silica and rather low on alkaline fluxes. I would expect it to be sort of short which is one of the observations about the kugler stuff.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #3  
Old 04-28-2019, 01:01 AM
Sean Jones Sean Jones is offline
Registered User
 
Join Date: Jan 2016
Location: Staffordshire U.K.
Posts: 16
Sean Jones is on a distinguished road
I asked them about Kugler but they feel that itís too expensive. This stuff is comparatively cheep. I only know itís Telux from the label on the bags it came in.
As a beginner I imagine I need a long glass. I can live with it eating the crucible, Iím making clay 40# pots which crack after 4 or 5 heats anyhow.
Reply With Quote
  #4  
Old 04-28-2019, 06:28 AM
David Schimmel David Schimmel is offline
Registered User
 
Join Date: May 2004
Location: Pennsylvania
Posts: 40
David Schimmel is on a distinguished road
I suspected it was in Germany and search for Telux Glas, instead of Telux glass and found Telux is located in Weisswasser, Saxony near the Polish border.

https://telux-glas.de/en/home
__________________
David Schimmel
Reply With Quote
  #5  
Old 04-28-2019, 08:53 AM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 290
Shawn Everette is on a distinguished road
What are you using for a furnace? Sounds like you're being pretty rough on the pots.

As far as working time, as long as you're not using bottle glass you should be fine. What's the price point on the Telux.
Reply With Quote
  #6  
Old 04-28-2019, 09:42 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,251
Pete VanderLaan is on a distinguished road
"Iím making clay 40# pots which crack after 4 or 5 heats anyhow."
******
Making your own pots is yet another artform. In England, Dyson pretty much has a monopoly unless you want to go on the continent and get Fafnir. Any pots I've ever made were kyanite and ball clay. They were great as long as you never turned the furnace off. Then? It's gone.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #7  
Old 04-28-2019, 04:17 PM
Sean Jones Sean Jones is offline
Registered User
 
Join Date: Jan 2016
Location: Staffordshire U.K.
Posts: 16
Sean Jones is on a distinguished road
I made my melter, it has as much Wire as I could get in and an SCR. An inch and a half from the elements to the crucible wall. 5Ē to 6Ē of frax, 4kW holds 20kg of glass.
I live in the potteries (Stoke on Trent) so pick up bags of heavily gorged stone ware originally produced for making saggers (the containers that protect pots in a kiln). T Material from Thermal Ceramics seems best but is about $70 a pot (10kg). The cheeper brands are about $25 a pot. Takes me a total of 2 hours to make a pot. To buy a pot Iím looking at $400.
The Telux cullet is $1 per pound (£1.50/kg in real numbers).
Reply With Quote
  #8  
Old 04-28-2019, 06:06 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,251
Pete VanderLaan is on a distinguished road
Keep your grog content high. Use any higher alumina clay compounds you can. Expect failure when you shut down, but not on just running. China clay is your friend. The cullet you are getting is a means to an end. . It's a tool. no more.

When you need better tools, it will likely come from a visit with a friend who opens your eyes.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #9  
Old 04-29-2019, 02:51 AM
Sean Jones Sean Jones is offline
Registered User
 
Join Date: Jan 2016
Location: Staffordshire U.K.
Posts: 16
Sean Jones is on a distinguished road
I think my pots die in the silica inversions on the way up. I once heard one crack in the middle of the crystobalite range. I take 53 hours to heat up, 5 deg/hour through cristobolite and 10 deg/hour through the quartz inversion.
The cracks are annular round the base. Iíve changed the shape to make the bottom more rounded and cut deep grooves in the plinth to allow more heat to get to the base.
We have a wood fired furnace we run for a week in summer. We have to let in cool somewhat between firings (we have to sleep) so I invest the bottom of the pot to stop it leaking. That seems to work well.
What temperature is it safe to drop down to for several days without devit?
Reply With Quote
  #10  
Old 04-29-2019, 09:29 AM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 290
Shawn Everette is on a distinguished road
Are you stilting your pot? If not that might be part of your cracking problem, bottom of the furnace pulling too much heat.

My up cycle it typically 4-7 days, but I've got a 500lb tank. There are some crucial hold step that I try to hit at 900, 1250, and 1600; so a few soak steps may help as well.

I've held tanks as low as 1550 without much issues, but devit is always dependent on your glass. Typically is I'm holding a tank for later I keep it about 1800, nice thorough squeeze and can be back up almost instantly.
Reply With Quote
  #11  
Old 04-29-2019, 10:07 AM
Sean Jones Sean Jones is offline
Registered User
 
Join Date: Jan 2016
Location: Staffordshire U.K.
Posts: 16
Sean Jones is on a distinguished road
Using stilts sounds like a good idea. Iíve not come across that before.
Your hold temperatures are also interesting. I assumed that once I was above the quarts inversion at 1070F I was safe to go up fast.
Reply With Quote
  #12  
Old 04-29-2019, 10:34 AM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 290
Shawn Everette is on a distinguished road
All free standing pots I've seen are stilted with hard brick, it allowed the heat discrepancy at the bottom of the pot to be not as drastic.

From my experience you want to take it slow to about 1500F. Quartz inversion is a key factor, but there is still changes happening past that point. I don't l know that the pots ever get to the full vitrification stage, but there has got to be shrink.

Another thing you may consider is a different furnace configuration. A frax design is going to be a complete heat dump no matter mow much you have. The SCR is going to help with maintaining accurate temps, but even soft brick is going to allow for much better heat retention and gentler cycle. Hard brick or castable would help even more, and will resist corrosion better. Frax is fine for holes or kilns, but furnaces should really be made from a denser material. There's an excellent chapter on R factor in Glassnotes.
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is Off
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 11:32 PM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2019, Jelsoft Enterprises Ltd.
© CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.