coloring clear glass

Can you add chunks of rods to clear cullet and melt in a small color pot to make colors? Maybe as powdered color mixed with clear powder and mix into wet cullet.
Franklin
Reply With Quote
  #2  
Old 01-23-2017, 10:04 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 19,813
Pete VanderLaan is on a distinguished road
Well, you can. That doesn't mean it will look good or anything remotely like it. With many colors, it won't be recognizable. Rolling it in the powder or cullet is your only realistic option.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #3  
Old 01-23-2017, 02:00 PM
Franklin Sankar's Avatar
Franklin Sankar Franklin Sankar is offline
Registered User
 
Join Date: Apr 2002
Location: Trinidad, West Indies
Posts: 3,682
Franklin Sankar is on a distinguished road
One color only per pot but I get your point
Franklin
Reply With Quote
  #4  
Old 01-23-2017, 03:23 PM
Eric Trulson Eric Trulson is offline
Young Turk
 
Join Date: Sep 2014
Location: NH
Posts: 70
Eric Trulson is on a distinguished road
I know it's been mentioned here a few times before, but saving your different color scrap (moils and any trashed pieces or cutoffs that have already had color applied) and melting it all together once you have a pot's worth tends to result in a nice light transparent blue.

Bit of a one trick pony (you're only ever going to get that one shade of blue, maybe a blue/green at most), and as Pete says, you're almost certainly better off saving any rod/frit/powder to use directly. It is a nice way to recycle glass scrap if you don't need perfect optical clarity though (I have yet to run one of those scrap melts without getting small bubbles and some cording).
Reply With Quote
  #5  
Old 01-23-2017, 04:31 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 19,813
Pete VanderLaan is on a distinguished road
I don't know why it's always blue, but it always is.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #6  
Old 01-23-2017, 06:23 PM
Cecil McKenzie Cecil McKenzie is offline
Registered User
 
Join Date: Feb 2011
Location: Emporia, KS
Posts: 461
Cecil McKenzie is on a distinguished road
Cobalt takes one part in 5000 to make a visible color. If you never used any cobalt color it would not be blue.
Reply With Quote
  #7  
Old 01-23-2017, 07:34 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 19,813
Pete VanderLaan is on a distinguished road
actually, one in ten thousand shows distinct color but it doesn't make it pretty. . Even so it always looks like faded blue jeans. Just ladle the heel.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #8  
Old 02-01-2017, 10:16 PM
rodman gilder miller rodman gilder miller is offline
Registered User
 
Join Date: Aug 2014
Location: seattle
Posts: 63
rodman gilder miller is on a distinguished road
The blues come through because the other colors are more radically concentration dependent: many of the yellows-orange-reds are a combo of selenium cadmium and sulfur. dilute it out a small amount and the color center doesn't form. Beer-bottle brown is sulfur and carbon combined . Copper and gold rubies have a colloidal color center with something like 1,000 to 5,000 atoms! We can expect that to be invisible with small dilutions. Cobalt and copper have colors which arise from a single atom in solution. They come through with a concentration dilution.
__________________
You have to dance with the glass
Reply With Quote
  #9  
Old 02-10-2017, 02:12 PM
Dennis Hetland Dennis Hetland is offline
Registered User
 
Join Date: Sep 2009
Location: Salem, OR
Posts: 304
Dennis Hetland is an unknown quantity at this point
I use scrap sp cullet. I can't help, but put some pieces that contain some color in the pot. All colors "burn off". Greens and blacks become blue.
Yellows and reds disappear. Why? I believe it's because my furnace has an oxidizing atmosphere. That would mean(unless I'm wrong) that the holes in the atomic lattice are being filled, which prevents the larger, slower, yellow and red wavelengths from being able to pass while still allowing the shorter, more powerful blue wavelengths to pass.
Light is thought of as being both a wave and a particle at the same time. That's why a "wave "would need a space/hole in the valence belt.
__________________
candlewoodglass@gmail.com

Last edited by Dennis Hetland; 02-10-2017 at 02:16 PM. Reason: spelling
Reply With Quote
  #10  
Old 02-10-2017, 04:29 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 19,813
Pete VanderLaan is on a distinguished road
Quote:
Originally Posted by Dennis Hetland View Post
All colors "burn off". .
*********
Actually, no they don't.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #11  
Old 02-14-2017, 05:07 PM
Dennis Hetland Dennis Hetland is offline
Registered User
 
Join Date: Sep 2009
Location: Salem, OR
Posts: 304
Dennis Hetland is an unknown quantity at this point
With the exception of blue that has been my experience.
__________________
candlewoodglass@gmail.com
Reply With Quote
  #12  
Old 02-14-2017, 06:40 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 19,813
Pete VanderLaan is on a distinguished road
Don't confuse dilution with ionization. Many colors rely on specific balances to show their color. Cobalt is not one of those elements. Neither is iron and both can show a blue color. Copper can show blue as well. Cobalt just happpens to show color at one part in 10,000. Manganese can have its color dissipate in a reducing atmosphere but I would not refer to it as burn out but as a valence shift. Selenium can be in five states of valence. Only one shows color. Cadmium only shows color in the presence of sulfur. Cerium and Titanium can show a yellow but only when both are present and in the right ratio. Copper in reduction is a red sometimes, in oxidation, a blue, or a green, sometimes a gray. But it's not burning out.
It is the case that loss can be measured in micrograms per hour of lead leaving a melt based on melt temps. It goes up as the temp goes up. I am not convinced yet that selenium volatilizes in an existing glass but I do beleive it changes valence easily. Again, those type losses are in micrograms per hour. Selenium volatilizing largely is deemed to occur in the batch melt, not in a cullet. My best understanding is that sodium does volatilize as well to a lesser degree. Your color rods require a very fixed concentration to show their color. Chucking them in the clear is going to make the color dissipate in the goop.
__________________
Where are we going and why am I in this basket?
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 12:54 AM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2018, Jelsoft Enterprises Ltd.
© CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.