Dying or coloring sandblasted glass

Hey All,
I'm new to this ( Thanks JB) I am hoping to color a large 3ft glass piece that I sandblasted ? I was hoping for a translucent coloration that was some how dipped in color or airbrushed ? I would love all and any suggestions on what paint to use , or techniques. Thanks for taking the time.
Reply With Quote
  #2  
Old 10-12-2018, 05:19 PM
Greg Vriethoff's Avatar
Greg Vriethoff Greg Vriethoff is offline
PotatoFish
 
Join Date: Jan 2007
Location: Charlotte, NC
Posts: 2,007
Greg Vriethoff is on a distinguished road
You can use various painting mediums to color sandblasted glass. Oil, acrylic, or watercolor all work. It depends on what the piece's final function is. Watercolor is not permanent. Acrylic has a short working time. Oil based media yields the most subtle and desirable results. Apply and then wipe to remove excess.

My experience is not extensive, but coupled with what I have seen from other artists I would go with oils.

I can't speak to airbrush or dyes.
__________________
"It's such a fine line between stupid and clever." - David St. Hubbins
Reply With Quote
  #3  
Old 10-12-2018, 05:28 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 20,598
Pete VanderLaan is on a distinguished road
Look to Joan Irving and the installation in the airport in San Diego.

Joan used enamel powders on her work to then be refired into the abraded areas.

Really well done.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #4  
Old 10-12-2018, 08:15 PM
Sky Campbell's Avatar
Sky Campbell Sky Campbell is offline
Registered User
 
Join Date: May 2002
Location: Gainesville FL
Posts: 893
Sky Campbell is on a distinguished road
I did two 5x8 panels heavily carved pierced with lamp worked branches and cherry blossoms. I tried oil paints and found them to dirty and fade over time. Ended up using pebeo paints. Airbrushed and fired to 325f. Looks as good today as when it was hung.
Attached Images
File Type: jpg image.jpg (68.2 KB, 62 views)
Reply With Quote
  #5  
Old 10-12-2018, 08:17 PM
Sky Campbell's Avatar
Sky Campbell Sky Campbell is offline
Registered User
 
Join Date: May 2002
Location: Gainesville FL
Posts: 893
Sky Campbell is on a distinguished road
I guess you can only load one attachment per post. That is just part of the design. Anyway you get the idea.
Reply With Quote
  #6  
Old 10-12-2018, 11:18 PM
Eben Horton Eben Horton is offline
Registered User
 
Join Date: Apr 2002
Location: Wakefield, RI
Posts: 4,402
Eben Horton is on a distinguished road
I have used this with great results.

https://decoart.com/glass-paint/education
__________________
<eben epoiese>
Reply With Quote
  #7  
Old 10-13-2018, 10:22 AM
Tom Fuhrman Tom Fuhrman is offline
Registered User
 
Join Date: Apr 2002
Location: hills of Tennessee
Posts: 1,377
Tom Fuhrman is on a distinguished road
I've had good luck with orasol dyes used in adhesives but I would think they could be put in a media and sprayed. The dyes were made by Ciba Geigy. They are fade resistant for 30-50 years depending upon color selection.
Reply With Quote
  #8  
Old 10-13-2018, 10:23 AM
Tom Bloyd Tom Bloyd is offline
Registered User
 
Join Date: Nov 2007
Location: Kansas city
Posts: 146
Tom Bloyd is on a distinguished road
That's a great close up of your piece Sky. Would love to see the whole image. Very cool!
Reply With Quote
  #9  
Old 10-13-2018, 11:15 AM
Dave Bross Dave Bross is offline
Registered User
 
Join Date: Apr 2002
Location: Archer FL(near Gainesville)
Posts: 2,949
Dave Bross is on a distinguished road
Rich or someone will probably remember who this was but someone in Seattle used to blow large transparent pieces and then paint them with One Shot sign paints.

The One Shot stuff is full of lead and I don't thing any are translucent.
__________________
Art is not a thing...it's a way.
Reply With Quote
  #10  
Old 10-13-2018, 12:10 PM
Rich Samuel's Avatar
Rich Samuel Rich Samuel is offline
Registered User
 
Join Date: Apr 2002
Location: Seattle, WA
Posts: 2,402
Rich Samuel is on a distinguished road
Dave, the only person who comes to mind is Bob Carlson, but I don't know what paints he used after (early on) giving up Testor model paints.
Reply With Quote
  #11  
Old 10-13-2018, 03:11 PM
Rosanna Gusler Rosanna Gusler is offline
Registered Fuser
 
Join Date: Mar 2003
Location: Wanchese, NC
Posts: 916
Rosanna Gusler is on a distinguished road
Alcohol inks would work.
Reply With Quote
  #12  
Old 10-13-2018, 03:29 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 20,598
Pete VanderLaan is on a distinguished road
Quote:
Originally Posted by Dave Bross View Post
Rich or someone will probably remember who this was but someone in Seattle used to blow large transparent pieces and then paint them with One Shot sign paints.

The One Shot stuff is full of lead and I don't thing any are translucent.
******
Cappy Thompson?
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #13  
Old 10-13-2018, 06:44 PM
Greg Vriethoff's Avatar
Greg Vriethoff Greg Vriethoff is offline
PotatoFish
 
Join Date: Jan 2007
Location: Charlotte, NC
Posts: 2,007
Greg Vriethoff is on a distinguished road
The drawback to using any type of oil-based media on sandblasted glass is its propensity to collect dust. Oil paint has a slow drying time, and accelerants can cause adhesion issues. Give 'em time to dry before setting it loose in the wild.

As to the issue of fading, lightfastness is always of concern with pigmentation whether we're talking about paints or dyes. It is of more concern if the object will be placed in direct sunlight. It has more to do with quality than application. You always get what you pay for. If you buy artist oils with, say, Rembrandt on the label the color is less likely to fade over time as opposed to ones with Bob Ross on them.
__________________
"It's such a fine line between stupid and clever." - David St. Hubbins
Reply With Quote
  #14  
Old 10-13-2018, 07:44 PM
Steven O'Day Steven O'Day is offline
Registered User
 
Join Date: Jun 2002
Location: portland oregon
Posts: 301
Steven O'Day is on a distinguished road
Danny Perkins, large blown and then painted. Don't recall what paint he uses.
Reply With Quote
  #15  
Old 10-13-2018, 08:25 PM
Randi Solin Randi Solin is offline
Registered User
 
Join Date: Oct 2018
Location: VT
Posts: 4
Randi Solin is on a distinguished road
Thanks so much for all your suggestions

I would upload a picture of the piece if I knew how to do that.
It is a 26" Magnolia bud with about 100 bits for the seed head.Lots of spots for coloration not to look uniform.
Reply With Quote
  #16  
Old 10-13-2018, 08:40 PM
Randi Solin Randi Solin is offline
Registered User
 
Join Date: Oct 2018
Location: VT
Posts: 4
Randi Solin is on a distinguished road
Thanks so much for all your suggestions

I would upload a picture of the piece if I knew how to do that.
It is a 26" Magnolia bud with about 100 bits for the seed head.Lots of spots for coloration not to look uniform.
Reply With Quote
  #17  
Old 10-14-2018, 08:12 AM
Rosanna Gusler Rosanna Gusler is offline
Registered Fuser
 
Join Date: Mar 2003
Location: Wanchese, NC
Posts: 916
Rosanna Gusler is on a distinguished road
I think that the paebo paints would be best for that. Edit... Traditional glass stainers colors would work as well look up Peter mcgrain . https://www.amazon.com/s/?ie=UTF8&ke...l_4ywjuc68f9_e

Last edited by Rosanna Gusler; 10-14-2018 at 08:16 AM. Reason: More thought
Reply With Quote
  #18  
Old 10-14-2018, 09:31 PM
Randi Solin Randi Solin is offline
Registered User
 
Join Date: Oct 2018
Location: VT
Posts: 4
Randi Solin is on a distinguished road
This is not a piece that can be brought back up in an anneiler. It's a no heat painting option but thank you.
Reply With Quote
  #19  
Old 10-14-2018, 10:15 PM
Max Epstein Max Epstein is offline
Registered User
 
Join Date: Sep 2016
Location: Tallahassee, FL
Posts: 232
Max Epstein is on a distinguished road
Not exactly what you're looking for, but it popped up in my feed.
Attached Images
File Type: jpg chihuly_acrylic_small.jpg (43.7 KB, 43 views)
Reply With Quote
  #20  
Old 10-17-2018, 05:48 PM
Marty Kremer Marty Kremer is offline
Registered User
 
Join Date: May 2004
Location: North Yarmouth ME
Posts: 446
Marty Kremer is on a distinguished road
Not a permanent exhibit, I suppose?
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is Off
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 04:41 AM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2019, Jelsoft Enterprises Ltd.
CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.