Worn jack blades

When I made my jacks I used mild steel for the blades. I wasnít sure there was any point in using carbon steel and hardening them as they were going to get hot in service which could re soften them.
Now I have a little experience I can see that they need to be ware resistant. Is it worth using manganese steel (if I can find it) or is mid/high carbon best. From the colour of my used pair Iíd guess it is worth hardening them as they donít appear to get hot enough to draw there temper and loose there hardness.
I know I shouldnít be grinding them on cold neck lines, Iím getting better at that.
Reply With Quote
  #2  
Old 11-20-2019, 12:10 PM
Eben Horton Eben Horton is online now
Registered User
 
Join Date: Apr 2002
Location: Wakefield, RI
Posts: 4,799
Eben Horton is on a distinguished road
This is just my opinion but you shouldnít judge a jack by its durability but by its workability. You want a set of blades that heat up quickly and hold wax.
Ivan Smith made his blades out of medium carbon Sheffield spring steel. He personally told me this.

If you blow glass properly you should not wear out your blades in your life time. The worst habit (and I have seen many English blowers do this) is to grab the punty rod with your jack blades to apply the punty to the bottom of your piece. This will wear your jacks out in a year of doing this on a regular basis.

If you make blades that are built to be durable the working properties of the steel on the glass may be less than favorable.
__________________
<EBEN EΠOIESEN >
Reply With Quote
  #3  
Old 11-20-2019, 12:53 PM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 696
Shawn Everette is on a distinguished road
If your jacks are getting hard enough to lose temper, you're doing it wrong. Medium steel should be fine, but Jim uses high and Jeff uses spring. Just remember to be nicer to your jacks that the other tools, your tweezers don't care what you do to them.
Reply With Quote
  #4  
Old 11-20-2019, 02:26 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,375
Pete VanderLaan is on a distinguished road
My best pair of jacks was made for me by Shorty Finley out of a leaf Spring on an old chevy. Those sadly vanished but they were light and held wax well.
I had a job at one point about 20 years back doing 800 weights and heavy vases for Washington Mutual. The weights were large and involved a hard jacking down off the punty. I wore a groove in the Moores and replaced them with Cutting Edge which have not worn at all. Of all of them, I really miss the one's Shorty made but a lot of that is probably sentimental.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #5  
Old 11-20-2019, 03:05 PM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 696
Shawn Everette is on a distinguished road
Jeff's materials and workmanship are top notch, but the ergo's always a little off for me. The angle the handles are set just seem too funky for me to want to get used to. If I had those demascus shears I might change my mind.

The Moore's have always fit my hand better, but they can get beat up easy. I have to fix shop sets every semester, but my personal set is working on 10+ years.

I won't bother to talk about essemce.
Reply With Quote
  #6  
Old 11-20-2019, 04:40 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,375
Pete VanderLaan is on a distinguished road
My first duck bills came from Essemce. Henry Summa wound up with them but they were wonderful compared to the stuff from Putsch, Jeff's duck bills continue to serve me well.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #7  
Old 11-20-2019, 07:50 PM
David Patchen's Avatar
David Patchen David Patchen is offline
Registered User
 
Join Date: Sep 2005
Location: San Francisco, CA
Posts: 1,914
David Patchen is on a distinguished road
There's a new glassblowing supply store opening in the UK called The Glass Toolbox; you can find them if you google. I'd recommend you see what commercially made jacks they carry and get a pair. The issue of jack blade material has been worked out (with varying degrees of success) and I bet any decent commercially-made jacks (Maruko, Jasen Johnsen, Carlo Dona, Jim Moore, Cutting Edge) are going to be better than what you make. That is unless you enjoy spending more time metalworking and less time glassblowing. Work hot and they won't wear much at all.
Reply With Quote
  #8  
Old 11-20-2019, 07:56 PM
Michael Ahlefeldt-Laurvig Michael Ahlefeldt-Laurvig is offline
Registered User
 
Join Date: Apr 2010
Location: Sweden
Posts: 882
Michael Ahlefeldt-Laurvig is on a distinguished road
Essemce jacks were the Volvos of jacks for me, after working in Japan I got the best from a Japaneese guy, absolutly beutiful, Ive never worn out any jacks in 29 years, and wheve run production
Reply With Quote
  #9  
Old 11-20-2019, 11:29 PM
Nick Delmatto Nick Delmatto is offline
Registered User
 
Join Date: Feb 2010
Location: Logan, OH
Posts: 67
Nick Delmatto is on a distinguished road
Quote:
Originally Posted by Pete VanderLaan View Post
My first duck bills came from Essemce. Henry Summa wound up with them but they were wonderful compared to the stuff from Putsch, Jeff's duck bills continue to serve me well.
A lot of first names thrown around.....who's Jeff?
Reply With Quote
  #10  
Old 11-21-2019, 07:55 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,375
Pete VanderLaan is on a distinguished road
Jeff Lindsay- Red Hot Metal, also known as Cutting edge.
Henry Summa.- first apprentice deceased
Shorty Findley- Gaffer at Blenko. Quite the character.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #11  
Old 11-21-2019, 08:34 AM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 696
Shawn Everette is on a distinguished road
Essemce aren't volvo, I loved my s80. I'd say maybe saab. They worked, but needed improvement, and you only really see them in shops as curios.
Reply With Quote
  #12  
Old 11-21-2019, 08:35 AM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 696
Shawn Everette is on a distinguished road
I really hope Jim doesn't need to be explained.
Reply With Quote
  #13  
Old 11-21-2019, 01:21 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,375
Pete VanderLaan is on a distinguished road
Quote:
Originally Posted by Shawn Everette View Post
I really hope Jim doesn't need to be explained.
****
You'd be surprised. Jim Moore, a fine toolmaker.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #14  
Old 11-22-2019, 04:15 AM
Michael Ahlefeldt-Laurvig Michael Ahlefeldt-Laurvig is offline
Registered User
 
Join Date: Apr 2010
Location: Sweden
Posts: 882
Michael Ahlefeldt-Laurvig is on a distinguished road
As in common, utilitarian, workhorse, students cant ruin them. Agree room for improvements
Reply With Quote
  #15  
Old 11-22-2019, 10:03 AM
Kenny Pieper Kenny Pieper is offline
Registered User
 
Join Date: Feb 2003
Location: Burnsville N.C.
Posts: 845
Kenny Pieper is on a distinguished road
Check these out. They were Walter Evens
Attached Images
File Type: jpg walters jacks.jpg (35.0 KB, 120 views)
Reply With Quote
  #16  
Old 11-22-2019, 05:53 PM
Scott Dunahee's Avatar
Scott Dunahee Scott Dunahee is offline
Registered User
 
Join Date: Apr 2002
Location: Madison, WI
Posts: 645
Scott Dunahee is on a distinguished road
That is awesome.

Awesome.

BSD
__________________
That's all right. I never expected there to be a blue light special on enlightenment...
Reply With Quote
  #17  
Old 05-28-2020, 02:39 AM
Sean Jones Sean Jones is offline
Registered User
 
Join Date: Jan 2016
Location: Staffordshire U.K.
Posts: 31
Sean Jones is on a distinguished road
I made a new pair of jacks with D6 blades, a ware resistant high chrome steel. Hardened the blades and tempered them to about 60 HRC (very hard and possibly a bit brittle).
The difference is remarkable. These have a much smoother feel. Especially as you squeeze down on a cooling neck line. You donít get that grinding feeling when youíve run out of heat. As yet, no dirty jack lines as Iím not leaving any steel behind.
I imagine they are going to last a long time.
Reply With Quote
  #18  
Old 05-28-2020, 08:23 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,375
Pete VanderLaan is on a distinguished road
Don't work your glass too cold and they will.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #19  
Old 06-01-2020, 12:31 AM
Jon Myers's Avatar
Jon Myers Jon Myers is offline
Registered User
 
Join Date: Apr 2002
Location: Portland OR
Posts: 631
Jon Myers is on a distinguished road
One of the most outstanding glass tools Iíve seen were Ed skeels diamond shears. D8 steel, double beveled and polished on the back of the blade so the only thing that really touched the glass was one point in the center of th3 V. And the v was more open than the cutting edge big shears by quite a bit and you could cut much bigger glass.
Reply With Quote
  #20  
Old 06-01-2020, 06:26 PM
Eric Trulson Eric Trulson is offline
Young Turk
 
Join Date: Sep 2014
Location: Stanwood, WA
Posts: 153
Eric Trulson is on a distinguished road
Quote:
Originally Posted by Jon Myers View Post
One of the most outstanding glass tools Iíve seen were Ed skeels diamond shears. D8 steel, double beveled and polished on the back of the blade so the only thing that really touched the glass was one point in the center of th3 V. And the v was more open than the cutting edge big shears by quite a bit and you could cut much bigger glass.
Man, I miss Ed. Went looking for one of his videos on youtube the other day, but his "Keith Orr" account and all the videos are all totally gone. Good toolmakers are thin on the ground, I wish he were still around.

(Incidentally, if anyone has a locally stored copy of that video showing the robot arm spinning out an enormous rondel, please let me know. That clip is just too good to let it get lost in the sands of time)
Reply With Quote
  #21  
Old 06-01-2020, 06:48 PM
Eben Horton Eben Horton is online now
Registered User
 
Join Date: Apr 2002
Location: Wakefield, RI
Posts: 4,799
Eben Horton is on a distinguished road
I miss Ed too. I mean... who else has cremated a cat in their gloryhole ?
__________________
<EBEN EΠOIESEN >
Reply With Quote
  #22  
Old 06-01-2020, 07:53 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,375
Pete VanderLaan is on a distinguished road
Ed is on the road with his truck. I hear from time to time. Truly a troubled soul.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #23  
Old 06-02-2020, 03:57 AM
Sky Campbell's Avatar
Sky Campbell Sky Campbell is offline
Registered User
 
Join Date: May 2002
Location: Gainesville FL
Posts: 1,026
Sky Campbell is on a distinguished road
Quote:
Originally Posted by Eric Trulson View Post
Man, I miss Ed. Went looking for one of his videos on youtube the other day, but his "Keith Orr" account and all the videos are all totally gone. Good toolmakers are thin on the ground, I wish he were still around.

(Incidentally, if anyone has a locally stored copy of that video showing the robot arm spinning out an enormous rondel, please let me know. That clip is just too good to let it get lost in the sands of time)
You can find all his videos in the Wayback machine under the old keith Orr website.
Reply With Quote
  #24  
Old 06-02-2020, 09:09 AM
Eben Horton Eben Horton is online now
Registered User
 
Join Date: Apr 2002
Location: Wakefield, RI
Posts: 4,799
Eben Horton is on a distinguished road
Back to the jack blades.
Shin @ Maruko tools just started making blades out of chrome vandium steel.
__________________
<EBEN EΠOIESEN >
Reply With Quote
  #25  
Old 06-02-2020, 05:23 PM
Larry Cazes Larry Cazes is offline
Registered User
 
Join Date: Feb 2006
Location: San Jose, CA
Posts: 1,024
Larry Cazes is on a distinguished road
Quote:
Originally Posted by Eben Horton View Post
Back to the jack blades.
Shin @ Maruko tools just started making blades out of chrome vandium steel.
been using their tweezers for a long time. My favorites
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is Off
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 09:13 AM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2021, Jelsoft Enterprises Ltd.
© CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.