White turning pink in annealer

Any idea what would cause an enamel white to turn pink in the annealer? If we drop the piece on the floor and it cools rapidly it is white?
Reply With Quote
  #2  
Old 05-22-2020, 01:58 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,925
Pete VanderLaan is on a distinguished road
I would have to imagine it's the arsenic Rich. There's nothing else in that formulation that would suggest color. Is it electric or gas annealing?
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #3  
Old 05-22-2020, 04:30 PM
Larry Cazes Larry Cazes is online now
Registered User
 
Join Date: Feb 2006
Location: San Jose, CA
Posts: 969
Larry Cazes is on a distinguished road
Gaffer had this issue years ago. At that time i remember it being batch related.
Reply With Quote
  #4  
Old 05-22-2020, 05:43 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,925
Pete VanderLaan is on a distinguished road
all the arsenates have the pinking issue. Striking in the lehr is somewhat extreme.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #5  
Old 05-22-2020, 06:29 PM
Larry Cazes Larry Cazes is online now
Registered User
 
Join Date: Feb 2006
Location: San Jose, CA
Posts: 969
Larry Cazes is on a distinguished road
Quote:
Originally Posted by Pete VanderLaan View Post
all the arsenates have the pinking issue. Striking in the lehr is somewhat extreme.
I distinctly remember gaffer discounting a batch of enamel because it struck to pink in the annealing.
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is Off
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 03:27 PM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2020, Jelsoft Enterprises Ltd.
CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.