Over the years I have piled up a couple hundred pounds of older color bars. Most are Kuglar and Zimmerman and 75% opaque. Most bars look like they are from the 80s and 90s. I understand only basics of color and Coe. I am currently running spectrum 2.0 nuggets. Looking for clues like surface applications? Mixing multi colors? Use with thicker pieces? Reheating issues?
Reply With Quote
  #2  
Old 10-25-2017, 08:33 PM
Josh Bernbaum Josh Bernbaum is offline
Registered User
 
Join Date: Feb 2009
Location: Brattleboro, VT
Posts: 656
Josh Bernbaum is on a distinguished road
If you ever consider selling any of those Zimmerman bars please give me
a shout. Fit-wise, I'd be most cautious with some of the Kuglers. Learn how to do some ring tests if you don't know already. There is a section in Glass Notes 4 (I think) that describes what you're looking for. And you can always ask here too.
Just a friendly heads up, but want to warn you someone around here tends to get miffed if you refer to it as "COE". Use L.E.C.
__________________
www.jmbglass.com
instagram.com/joshbernbaum_glass
Reply With Quote
  #3  
Old 10-26-2017, 08:27 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,571
Pete VanderLaan is on a distinguished road
Kugler opaques virtually all have Linear expansion coefficients from 89 on down to 85. They are not going to really fit a glass with a 96 linear expansion coefficient. Zimmermann made some incredibly beautiful colors. The mother of pearl colors are going to cause problems. Spruce Pine made SP83 specifically to address this issue.

I just took a nice little lithium pill.
__________________
Where are we going and why am I in this basket?
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 07:35 AM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2020, Jelsoft Enterprises Ltd.
CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.