Lino's Nero Tea

That's what we called it at Manifesto anyway.

Sand 100
Soda 44
Calcium 16
Boric Acid 3
Sulphur 3.950
Rosin 1.3
Iron Oxide 2.850
Black Nickle Oxide 1

Just for cane or threading. Overlay onto gaffer duro white for extra opaqueness in those super stretched out cane pick ups. Fun to melt. Not as bad as Pete would have you believe

Have fun kids.
__________________
WWUD? Think for yourself.
Reply With Quote
  #2  
Old 12-22-2016, 02:32 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,268
Pete VanderLaan is on a distinguished road
Quote:
Originally Posted by Jordan Kube View Post
. Not as bad as Pete would have you believe

Have fun kids.
*********
Indeed, and the reason they named it that is that when you quenched it in water, the water turned black. I remember the rosin blacks. They lit on fire.
Yum...There are way worse things to make. Furthermore it used real "Sulphur", none of this candy ass "sulfur" you see sold on street corners in Eugene.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #3  
Old 11-06-2017, 12:39 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,268
Pete VanderLaan is on a distinguished road
well, good ventilation will make it less of a problem. That's the stuff.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #4  
Old 11-06-2017, 03:03 PM
Eben Horton Eben Horton is offline
Registered User
 
Join Date: Apr 2002
Location: Wakefield, RI
Posts: 4,776
Eben Horton is on a distinguished road
What is Rosin?
Reply With Quote
  #5  
Old 11-06-2017, 04:43 PM
Eric Trulson Eric Trulson is online now
Young Turk
 
Join Date: Sep 2014
Location: Stanwood, WA
Posts: 152
Eric Trulson is on a distinguished road
Quote:
Originally Posted by Eben Horton View Post
What is Rosin?
It's a purified form of pine sap/pitch. You make it by dissolving pitch in a solvent like acetone, then slowly heating the solution up until all the acetone and pine terpenes have vaporized. Changes from a thick sticky liquid into a slightly waxy solid.

Link for purchase: https://www.amazon.com/Lb-Powdered-P.../dp/B00LFPRS0O
Reply With Quote
  #6  
Old 11-06-2017, 04:57 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,268
Pete VanderLaan is on a distinguished road
It looks to be a reasonable source. I used to get it as rosin bags in sporting goods stores.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #7  
Old 11-06-2017, 05:44 PM
Greg Vriethoff's Avatar
Greg Vriethoff Greg Vriethoff is offline
Registered User
 
Join Date: Jan 2007
Location: Charlotte, NC
Posts: 2,244
Greg Vriethoff is on a distinguished road
It's also traditionally used in cake form on bows for stringed instruments (violins, cellos, etc.).

http://www.musiciansfriend.com/orche...natural-rosin/
__________________
Temperature and time.
Reply With Quote
  #8  
Old 11-06-2017, 06:41 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,268
Pete VanderLaan is on a distinguished road
Quote:
Originally Posted by Greg Vriethoff View Post
It's also traditionally used in cake form on bows for stringed instruments (violins, cellos, etc.).

http://www.musiciansfriend.com/orche...natural-rosin/
*********
It does but rosin for the bow is usually in a solid form and hard to mix in a batch.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #9  
Old 11-06-2017, 07:26 PM
Eben Horton Eben Horton is offline
Registered User
 
Join Date: Apr 2002
Location: Wakefield, RI
Posts: 4,776
Eben Horton is on a distinguished road
What purpose does it serve in the glass? a reducing agent?
Reply With Quote
  #10  
Old 11-07-2017, 07:37 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,268
Pete VanderLaan is on a distinguished road
If you must know:
C15.H20.06
Seems quite the popular go to substance for making hash. In Glass its got lots of Carbon to burn, so I'd say reduction. Not quite sure about the catching on fire beyond all that carbon, hydrogen and oxygen. That's H 20, not H2O as near as I can see. Big difference.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #11  
Old 11-07-2017, 08:21 AM
Eben Horton Eben Horton is offline
Registered User
 
Join Date: Apr 2002
Location: Wakefield, RI
Posts: 4,776
Eben Horton is on a distinguished road
Thanks for explaining... that’s an interesting ingredient.
Reply With Quote
  #12  
Old 03-20-2019, 12:46 PM
Bradley Howes Bradley Howes is offline
Registered User
 
Join Date: Mar 2015
Location: Alfred University
Posts: 62
Bradley Howes is on a distinguished road
I did a quick calculation to see what the conversion of rosin to sugar would be. I don't know if sugar would be a suitable substitute though. Based on the amount of carbon in both rosin and sugar, for 1.3 of rosin, use 1.8g cane sugar. Sugar from beets would have a different amount because there's a different amount of carbon per molecule of sugar.
Reply With Quote
  #13  
Old 03-20-2019, 12:49 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,268
Pete VanderLaan is on a distinguished road
I'd be inclined to avoid changing something you have yet to melt. Try to get some rosin. Sporting goods stores will have bags for pitchers and music stores would have it for bows on string instruments. I would imagine google would turn up sourcing.
If Lino used rosin, he had good reason to. Sugar was not hard to find.

Here's a rosin source, I suspect expensive but a start. Crush it.

https://www.amazon.com/Buck-Sticky-R...&hvrand=136956

When you look at classic recipes, they're classic for a reason and stood the test of time. If you want to change the world, that's really OK but you need a place to stand. I recommend standing with tradition. Go from there. Try this goop. Melt it. report back. Take feedback. melt some more and begin your changes. I started with the encyclopedia Britannica fifty years back. It was a lot more lonely then with Dudley Giberson holding a light on the path. I just continue to think that the belief that you will break new ground this week is unlikely, particularly if you are just now inquiring about incompatibility. This actually is a long rocky road filled with silica stones.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #14  
Old 03-21-2019, 08:39 PM
Jordan Kube Jordan Kube is offline
?
 
Join Date: Aug 2003
Location: Seattle, WA
Posts: 1,715
Jordan Kube is on a distinguished road
A little cheaper: http://www.diamondgforestproducts.co...-rosin/186879/
__________________
WWUD? Think for yourself.
Reply With Quote
  #15  
Old 03-22-2019, 09:38 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,268
Pete VanderLaan is on a distinguished road
Thanks Jordan. I copied the link to classified ads. I have to wonder out loud how glycerine would work in this.
South Georgia must be nirvana for resin. We get all our fire starters from there. They must whack up a bazillion lbs a year for the purpose.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #16  
Old 03-22-2019, 03:48 PM
Mitcheal Veenstra Mitcheal Veenstra is offline
Registered User
 
Join Date: Apr 2002
Location: Arlington, Texas
Posts: 131
Mitcheal Veenstra is on a distinguished road
Using rosin in the batch pile instead of sugar could also be about when it puts things in reduction. It has a different flash point that sugar does. That's why sometimes in some formulas you'll see sugar used alongside rosin. It keeps the batch pile in reduction longer as things fire off at different rates/temps. I'd tend to agree with Pete about not changing a formula you haven't melted yet.
__________________
so much to learn.. so little time to learn it....
Reply With Quote
  #17  
Old 03-23-2019, 06:43 PM
Jordan Kube Jordan Kube is offline
?
 
Join Date: Aug 2003
Location: Seattle, WA
Posts: 1,715
Jordan Kube is on a distinguished road
Great observation Mitcheal.
__________________
WWUD? Think for yourself.
Reply With Quote
  #18  
Old 04-15-2019, 05:29 PM
Dave Bross Dave Bross is offline
Registered User
 
Join Date: Apr 2002
Location: Archer FL(near Gainesville)
Posts: 2,953
Dave Bross is on a distinguished road
I agree with Mitch.

The experiments I did with sugar had the reduction fading away quickly.
__________________
Art is not a thing...it's a way.
Reply With Quote
  #19  
Old 04-15-2019, 05:44 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,268
Pete VanderLaan is on a distinguished road
If you want instant fade, try silicon carbide. Here... and gone. A lot of foaming cleanser left in its wake.
__________________
Where are we going and why am I in this basket?
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 12:40 AM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2021, Jelsoft Enterprises Ltd.
© CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.