What is the secret to 3 color ribbon cane?

We are trying to make some ribbon cane for ornaments - white in the center and a transparent color on either side, so my questions are:
How to set it up? Flatten the white on a punty and add the color on either side or build the color on the punty As a color stack, switch axis to another runty and then flatten? How much color compared to the white? Equal parts?
Once all is ready to pull, twist less pull more?
Am I overthinking this?
Happy Thanksgiving!
First attempts attached even though its a lousy pic
Attached Images
File Type: jpg 3C66A70A-52E6-4018-82D9-B1507AA96ADF.jpg (61.6 KB, 70 views)
Reply With Quote
  #2  
Old 11-21-2018, 10:35 PM
Eben Horton Eben Horton is offline
Registered User
 
Join Date: Apr 2002
Location: Wakefield, RI
Posts: 4,421
Eben Horton is on a distinguished road
Make a white tongue and put colored bits on the side. Heat it pretty good to melt away the seams but if you canít get rid of the seams, just take a small gather and chase the air pockets back to the moil.

I use a drill to twist. The tighter the better.
__________________
<eben epoiese>
Reply With Quote
  #3  
Old 11-22-2018, 08:30 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 20,659
Pete VanderLaan is on a distinguished road
I heat up enamel white on a punty and then squish it so it looks like a lollipop.
Then color is applied to either side of the lollypop and squished yet again. Then, go into your clear pot with the thing straight up and down to keep bubbles out and gather the clear you want. Shape that up keeping the clear pushed towards the punty rod.

Since I do this stuff alone, I pull it in small segments at the bench, knock that off the punty wash rinse repeat. I make a lot of cane for Mary Beth's jewelry.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #4  
Old 11-22-2018, 10:00 AM
Kenny Pieper Kenny Pieper is offline
Registered User
 
Join Date: Feb 2003
Location: Burnsville N.C.
Posts: 819
Kenny Pieper is on a distinguished road
here is a little trick...once you have the tong shape white with the colors on the outside, heat it a bit cool the end then grab the end with something and twist 3/4 of a turn in the direction you will be twisting so it looks like a corkscrew. Now when you gather screw your way into the glass slowly. This way when you come out with the gather and marver it wont be like having a flat tire.
Reply With Quote
  #5  
Old 11-25-2018, 07:31 AM
Pringle Teetor's Avatar
Pringle Teetor Pringle Teetor is offline
Registered User
 
Join Date: Jul 2003
Location: Chapel Hill, NC
Posts: 638
Pringle Teetor is on a distinguished road
Thanks! I made some Friday and used about the same sized chunks this time, made the lollipop instead of a rectangle and it worked nicely. I wanted to try the corkscrew but my dyslexia gave me pause on which direction to turn. Maybe it doesnít matter?
Reply With Quote
  #6  
Old 11-25-2018, 07:58 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 20,659
Pete VanderLaan is on a distinguished road
It matters.
__________________
Where are we going and why am I in this basket?
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is Off
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 01:36 AM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2019, Jelsoft Enterprises Ltd.
© CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.