  #1  
Old 04-04-2019, 09:54 AM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 289
Shawn Everette is on a distinguished road
Degassing inside paperweights

So I've been working on some new paperweight designs, pretty basic disk of color in the center encased, and have been having issues with bubbles appearing where the color is. Now the odd thing that's been occurring is that the bubbles start to appear as I'm flashing the piece down. No fuzz, no scuzz, while working it, but a film builds on both sides of the color as the center starts to cool. I've tried it with multiple colors (mostly reichenbach) with the same result.

I've had plenty of gathered bubbles disappear on me as a piece gets cold, but never anything like this. Clues?
Attached Images
File Type: jpg IMG_20190404_104754925.jpg (48.3 KB, 70 views)
File Type: jpg IMG_20190404_104805090.jpg (45.2 KB, 67 views)
Reply With Quote
  #2  
Old 04-04-2019, 02:23 PM
Eben Horton Eben Horton is offline
Registered User
 
Join Date: Apr 2002
Location: Wakefield, RI
Posts: 4,537
Eben Horton is on a distinguished road
Itís a vacuum. Cool it down in a more gentle way and I bet they go away. When you flash it, the surface is expanding and pulling away at the gooey core which causes a vacuum bubble to appear.
__________________
<eben epoiese>
Reply With Quote
  #3  
Old 04-04-2019, 03:41 PM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 289
Shawn Everette is on a distinguished road
Makes sense. I've done these before, think I was using cristalica rather than studio nuggets, and it didn't happen. Also seems to be more frequent when I bother to punty the weight to clean up the pipe mark.
Reply With Quote
  #4  
Old 04-05-2019, 04:03 PM
Rick Kellner Rick Kellner is offline
Registered User
 
Join Date: Jan 2004
Location: Hillsboro, OR
Posts: 174
Rick Kellner is on a distinguished road
Gotta spin it into a selling point. Whip up a marketing spiel about thousands of little silver galaxies inside your universe globes. Proprietary technique, you know! Could wind up being your serendipitous paperweight accident.
Reply With Quote
  #5  
Old 04-05-2019, 10:27 PM
Jordan Kube Jordan Kube is offline
?
 
Join Date: Aug 2003
Location: Seattle, WA
Posts: 1,683
Jordan Kube is on a distinguished road
Quote:
Originally Posted by Rick Kellner View Post
Gotta spin it into a selling point. Whip up a marketing spiel about thousands of little silver galaxies inside your universe globes. Proprietary technique, you know! Could wind up being your serendipitous paperweight accident.
And then one day it doesn't work and you can't figure out how to reproduce it!
__________________
WWUD? Think for yourself.
Reply With Quote
  #6  
Old 04-06-2019, 07:19 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,247
Pete VanderLaan is on a distinguished road
So, Collectors reserve! Limited edition! Signed by the artist!
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #7  
Old 04-06-2019, 09:31 AM
Art Freas Art Freas is offline
Registered User
 
Join Date: Aug 2014
Location: Washington
Posts: 558
Art Freas is on a distinguished road
Paperweight with patented space vacuum inside.
Reply With Quote
  #8  
Old 04-06-2019, 09:44 AM
Mark Rosenbaum's Avatar
Mark Rosenbaum Mark Rosenbaum is offline
Registered User
 
Join Date: Apr 2002
Location: New Orleans, LA
Posts: 1,035
Mark Rosenbaum is on a distinguished road
I just tell people that there is a little bit of New Orleans air and "magic" in each one!
Reply With Quote
  #9  
Old 04-06-2019, 10:30 AM
Eben Horton Eben Horton is offline
Registered User
 
Join Date: Apr 2002
Location: Wakefield, RI
Posts: 4,537
Eben Horton is on a distinguished road
Quote:
Originally Posted by Mark Rosenbaum View Post
I just tell people that there is a little bit of New Orleans air and "magic" in each one!
And maybe their grandma
__________________
<eben epoiese>
Reply With Quote
  #10  
Old 04-06-2019, 11:52 AM
Mark Rosenbaum's Avatar
Mark Rosenbaum Mark Rosenbaum is offline
Registered User
 
Join Date: Apr 2002
Location: New Orleans, LA
Posts: 1,035
Mark Rosenbaum is on a distinguished road
Quote:
Originally Posted by Eben Horton View Post
And maybe their grandma
That's a different thread!
Reply With Quote
  #11  
Old 04-10-2019, 10:17 AM
Bradley Howes Bradley Howes is offline
Registered User
 
Join Date: Mar 2015
Location: Palo Alto, CA
Posts: 58
Bradley Howes is on a distinguished road
Jacob Willcox had an old piece of r-54 from chihuly's studio. He told me he was instructed to flash it before gathering to prevent bubbles from appearing later while working it. I don't know when these bubbles show up though. Maybe thats something to try?
Reply With Quote
  #12  
Old 04-10-2019, 10:28 AM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 289
Shawn Everette is on a distinguished road
I can always try, but I'm pretty thoroughly cooking it prior to gathering. I've gotten into the habit of at least heating once before gathering to cook of any dust from the marver or block skuz.
Reply With Quote
  #13  
Old 04-10-2019, 05:50 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,247
Pete VanderLaan is on a distinguished road
my mental jury is still out. Dust from whatever source is in my mind.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #14  
Old 04-13-2019, 07:18 AM
Eben Horton Eben Horton is offline
Registered User
 
Join Date: Apr 2002
Location: Wakefield, RI
Posts: 4,537
Eben Horton is on a distinguished road
Quote:
Originally Posted by Pete VanderLaan View Post
my mental jury is still out. Dust from whatever source is in my mind.
Perhaps it could be from block carbon - I.e. blocking too dry. But I still think it has to do with rapid cooling.
__________________
<eben epoiese>
Reply With Quote
  #15  
Old 04-13-2019, 07:57 AM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 289
Shawn Everette is on a distinguished road
I'd have more faith in the dust/carbon contaminate theory if the bubbles showed up after I gathered, not at the coldest point on the pipe.

I'm not really sure how to about cooling it slower. We've been flashing them down and not trying to speed it up with air or anything. Had the thought of blasting it with the torch. Next time we do them I might try to get pics/vid of them forming.
Reply With Quote
  #16  
Old 04-15-2019, 01:37 PM
rodman gilder miller rodman gilder miller is offline
Registered User
 
Join Date: Aug 2014
Location: seattle
Posts: 68
rodman gilder miller is on a distinguished road
Much ado about nothing... it is little pieces of vacuum. Consider a sphere of glass with a tough skin which is hard enough to resist shrinking. Inside is an area which is still hot enough to move and contract. Surface tension will resist formation of a bubble, but once a bubble starts, it will grow.

There is a lot of residual stress in such a paperweight, but that is OK because if the weight is symmetric, the stresses act to temper the glass.

Much ado about nothing
__________________
You have to dance with the glass
Reply With Quote
  #17  
Old 04-15-2019, 02:08 PM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 289
Shawn Everette is on a distinguished road
Considering that unwanted bubbles are a bane of many a glassblower, I'd say it at least a little ado about something. I get the concept of what is happening, I'm looking for suggestions to prevent it. I've done this work before with different glass and not had anything like this. If it was as ubiquitous as hot glass inside cold glass makes a vacuum then it should be in nearly all paperweights.
Reply With Quote
  #18  
Old 04-15-2019, 04:48 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,247
Pete VanderLaan is on a distinguished road
Back when Lenny DiNardo was making his grall work with overlays and not getting the kind of bubble you suggest, he said "Scrub the shit out of it". That at the time seemed dubious but I would tend to give it a second look. Joints between interfaces are chock full of mysteries but gas is usually a gas and it's made from the materials around us. I'd try cleaning stuff a lot more religiously. It just won't be fun. I don't tend to think its coming out of solution. viscosity is possible. In making color rods, when we slowed down the cooling process, things got a lot better. Give it three slow cooling heats before the box.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #19  
Old 04-15-2019, 04:49 PM
Dave Bross Dave Bross is offline
Registered User
 
Join Date: Apr 2002
Location: Archer FL(near Gainesville)
Posts: 2,954
Dave Bross is on a distinguished road
Remember those bubbles that went into solution when you fined the glass?

Think along the lines of what might be bringing them back.

As for the variation between glasses?

Depending on formulation, some glasses can suck up more of the things that were in those bubs before they found their way into the liquid state...and then bring them back to visit when least expected. The chemical makeup of the gas in the bubbles will be different from one glass brand to the next too.
__________________
Art is not a thing...it's a way.
Reply With Quote
  #20  
Old 04-15-2019, 04:53 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,247
Pete VanderLaan is on a distinguished road
I don't tend to think that gas which is absorbed back into solution is going to constantly come back unless the valence has switched on the outer electron ring of two specific elements, Arsenic and Antimony. I don't see that temp/valence switch happening here.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #21  
Old 04-15-2019, 05:43 PM
Dave Bross Dave Bross is offline
Registered User
 
Join Date: Apr 2002
Location: Archer FL(near Gainesville)
Posts: 2,954
Dave Bross is on a distinguished road
Good point.

Could a high internal vacuum change the valence switch temp?
__________________
Art is not a thing...it's a way.
Reply With Quote
  #22  
Old 04-16-2019, 09:07 AM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 289
Shawn Everette is on a distinguished road
I can try scrubbing the frit, but it just seems unnecessary. It seems odd that the base glass is essentially having a reaction to the color when it is solid, and not when it is blown. Also, doesn't happen when the color is away from the direct center. I'm doing another batch this morning, try to see how many flashes it takes to get the center of the glassy pop.
Reply With Quote
  #23  
Old 04-16-2019, 09:29 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,247
Pete VanderLaan is on a distinguished road
Back when we were doing the color rod business when we made fluorine opaques, the glass drew from the furnace as a total transparent and struck as it cooled- very rapidly but you could easily see whether there were bubbles in the gathers. We made the rod, hung it up until rigid and boxed it.

The next day, I would take samples of colors and run them through the diamond saw on the vertical, sawing the rod in half like a pickle might be sliced and there, in the core, the rod was laced with huge bubbles, not a few, fifteen or twenty per rod like swiss cheese.

So I changed the technique and after the rod was formed, I heated it in the gloryhole three times just to the point of it slumping and then cooled it again. Three heats, three cools. Then, it went into the box.

Testing those rods yielded absolutely no bubbles at all. It needed to be cooled throughout.

It's your call.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #24  
Old 04-16-2019, 11:44 AM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 289
Shawn Everette is on a distinguished road
So the batch I did today I got no irregular bubbles, despite not changing much about the way I flashed down. The main change was that I didn't punty any of them for clean up. One I'm going to cold work, but the other two I switched my axis before the last gather to get the face of the design oriented where I wanted, and poof, no bubble dusting.

This would make me think that it was a cold core and then reheating to clean up the surface after that was leading to the bubbles, not a hot core and cold surface.

I'm not sure if we can manage the switch prior the last gather for the main design my partner is working on, but so far the solution I've come to is don't punty the paperweight.
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is Off
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 04:42 PM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2019, Jelsoft Enterprises Ltd.
© CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.