Spreadsheet additions?

I've just put together a spread sheet for calculating L.E.C. (I know; its a guide not gospel) Is anyone willing to share any additional expansion values for things like strontium, or any other potentially useful ingredients, beyond what's listed in 'Modern Glass Practice' and 'Glass Notes IV'? Or have a suggestion of where to look for such additional values? Thanks in advance.
P.S. the original E&T values were published in 1927 in the Journal of the American Ceramic Society volume 10, pg. 551. It's a well written piece of history.
Reply With Quote
  #2  
Old 11-09-2019, 11:19 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 24,079
Pete VanderLaan is on a distinguished road
Look at Appen.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #3  
Old 11-09-2019, 10:15 PM
Josh Bernbaum Josh Bernbaum is online now
Registered User
 
Join Date: Feb 2009
Location: Brattleboro, VT
Posts: 921
Josh Bernbaum is on a distinguished road
I think Dave Bross mentioned here somewhere that strontium and barium were very similar on expansion factor. So I've been entering the strontium in the barium line of the spreadsheet. How accurate that is, I'm not sure yet but is what I've been doing on the spreadsheet for these phosphates I'm doing now which have a decent amt. of strontium.
__________________
www.jmbglass.com
instagram.com/joshbernbaum_glass
Reply With Quote
  #4  
Old 12-24-2020, 01:38 PM
Dave Bross Dave Bross is offline
Registered User
 
Join Date: Apr 2002
Location: Archer FL(near Gainesville)
Posts: 3,045
Dave Bross is on a distinguished road
Yup, what Josh said, I've got Barium at 1.40 and Strontium at 1.38.

One other you might not have, Phosphorous, P2O5, I have at .667

What's interesting to me is that as long as you're close, and you don't change the values for anything in the spreadsheet over time, your corrections getting to a match will take care of minor, and some major errors.

My opinion of the single most valuable aspect of a spreadsheet is in making those corrections to get a match with minimum tries.
__________________
Art is not a thing...it's a way.
Reply With Quote
  #5  
Old 12-24-2020, 04:25 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 24,079
Pete VanderLaan is on a distinguished road
that's interesting with the phosphate. It suggests a negative factor except that you can't just add P205. It needs to be attached to something which would throw the factor off. It is worth noting that calcium has a pretty low factor and that helps explain why one could add up to 5% cal phosphate without mismatch.

Of course then there are the ryolite stones.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #6  
Old 03-07-2021, 07:47 PM
Dave Bross Dave Bross is offline
Registered User
 
Join Date: Apr 2002
Location: Archer FL(near Gainesville)
Posts: 3,045
Dave Bross is on a distinguished road
I wrote it that way because the spreadsheet I made breaks every material into it's components then E&T factors each individual component.
__________________
Art is not a thing...it's a way.
Reply With Quote
  #7  
Old 07-18-2021, 04:25 PM
Jed Hannay Jed Hannay is online now
Registered User
 
Join Date: Jan 2007
Location: Charlottesville, Virginia
Posts: 10
Jed Hannay is on a distinguished road
Quote:
Originally Posted by Paul Stout View Post
I've just put together a spread sheet for calculating L.E.C. (I know; its a guide not gospel) Is anyone willing to share any additional expansion values for things like strontium, or any other potentially useful ingredients, beyond what's listed in 'Modern Glass Practice' and 'Glass Notes IV'? Or have a suggestion of where to look for such additional values? Thanks in advance.
P.S. the original E&T values were published in 1927 in the Journal of the American Ceramic Society volume 10, pg. 551. It's a well written piece of history.
I've got Strontium down as 1.6 in the Appen Factors.

Appen plays out better for me than E&T, delivering estimates that look like the imaginary numbers I'm looking for and track ok with reasonable percent component changes. Lithium tracks better an Appen for me in particular.

Here's a bloc of numbers for common components related to the Appen estimates if you'd like to run your numbers through it. There's many additional oxides in the Appen list that I've excluded for simplicity. B2O3 requires a proportion subcalc but it's probably -.5 in SLS glasses. (I could be wrong. )

Oxide Molecular Weight Appen Factor
SiO2 60.08 / 0.38
Al2O3 101.96 / -0.3
B2O3 69.62 / -0.5
Li2O 29.87 / 2.7
Na2O 61.97 / 3.95
K2O 94.2 / 4.65
CaO 56.08 / 1.3
MgO 40.31 / 0.6
ZnO 81.37 / 0.5
SrO 103.62 / 1.6

"Calculating" is a strong word. It's an estimate, but it's an estimate that gives you something to think about relative to whatever other testing parameters you employ.
Reply With Quote
  #8  
Old 12-18-2021, 06:29 PM
Andrew Horch Andrew Horch is offline
Registered User
 
Join Date: Oct 2018
Location: Seattle WA
Posts: 17
Andrew Horch is on a distinguished road
Has anyone tried to combine thermal expansion coefficients from difference sources? I found a website with thermal coefficients for a lot of materials at 25C ( https://www.msesupplies.com/pages/li...ered-materials ). I correlated the MSE 25C coefficients with Appen 400C ( https://glassproperties.com/expansio...ion-Models.htm ) and some other numbers I have. I got a very good correlation. Extrapolating from 25C to 400C is a big jump, but they do correlate well. I am not talking about using the MSE numbers directly, but either scaling the numbers or finding something that is roughly equivalent and do a 1:1 replacement. The goal is not perfection, but to get close enough that it only takes a few runs to achieve compatibility. Is using 25C data a reasonable starting point or is it a waist of time to use the low temp coefficients for anything?
Reply With Quote
  #9  
Old 12-18-2021, 06:53 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 24,079
Pete VanderLaan is on a distinguished road
try to stick to 19-300C and avoid the apples and oranges.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #10  
Old 12-18-2021, 07:09 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 24,079
Pete VanderLaan is on a distinguished road
Go try out your theories. Make some glass bodies based on your concepts. Glass has an interesting way to make plain whether things are working or not.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #11  
Old 02-01-2023, 10:27 PM
Ron Mynatt Ron Mynatt is offline
Registered User
 
Join Date: Apr 2008
Location: Springdale Arkansas
Posts: 195
Ron Mynatt is on a distinguished road
Where would I find a copy of Appen
Reply With Quote
  #12  
Old 02-02-2023, 09:33 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 24,079
Pete VanderLaan is on a distinguished road
I got mine out of Vargin on enamels. I'll poke around for another source.It shouldn't be hard.
Maybe in Volf? It sure does not show up obviously in a goggle search.
__________________
Where are we going and why am I in this basket?
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 11:36 AM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2023, Jelsoft Enterprises Ltd.
© CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.