Dark Bottle Green Recipe

Hi there! It's been an awfully long time since I was here, but thought I would ask a question. I hope everyone is doing well!

Does anyone have any recommendations for a dark bottle green recipe? We melt Gaffer Batch here at the Canberra Glassworks. I have a recipe for a tealy-green but it is not dark enough.

Per batch of 100kg it is:

Iron 500g
Cobalt 1g
Nic 1g
Copper 20g

I saw this thread from 2014:
http://talk.craftweb.com/showthread....n+glass+recipe

I have attached an image of the density we're after as inspiration. I have also attached some pics of samples of teal greens that we already melt, they're too light. Any suggestions? How about this one below?

Olive Green Bottle Glass
sand 100 kilos
potassium chromate 500 grams
manganese dioxide 1500 grams

If anyone has any recommendations that would be wonderful.
Thank you!
Attached Images
File Type: jpg Dark Green inspiration.jpg (43.2 KB, 54 views)
File Type: jpg Light Teal Green.jpg (22.7 KB, 45 views)
File Type: jpg Light Lagoon Green.jpg (24.0 KB, 44 views)
Reply With Quote
  #2  
Old 09-17-2020, 09:26 AM
Josh Bernbaum Josh Bernbaum is offline
Registered User
 
Join Date: Feb 2009
Location: Brattleboro, VT
Posts: 730
Josh Bernbaum is on a distinguished road
I'd first remove the copper. I don't think that's helping you any.
I have only done light/bright greens with chrome, with iron, and with vanadium. The base batch you're adding to will vary what effects you can expect from the colourants in most cases.
What I would think about trying if doing this myself would be chrome or iron with a bit of nickel maybe? And it'd be a trial-and-error, no way around it, to get to the concentrations that look the best. I like to do small test melts if I have time, which quickly give you a decent sense of the final colour after the batch goes flat in the furnace, although things do darken up a bit in my experience after the full melt/fining process. If you melt 2-5 kilos at a time, then it's easy to multiply for a larger melt later. The chrome and manganese may start getting a bit too brown/ugly-violet for you, because the chrome will 'activate' the manganese and make it have a stronger effect. But perhaps a little bit of manganese with the chrome will steer you towards a darker shade versus the nickel I mentioned. I think whether Gaffer's batch has any potassium in there, or just sodium, might come into play regarding that. Be careful with the chrome, but grind it up in a coffee grinder (Pete's trick) if it's the dichromate form, to get it into a fine powder vs. lumps. And don't skimp on the melt temp to help it go into solution and not form corundum flecks. It may also be the case that all you need is a boatload of chrome to get it to darken up the usually bright green shade it produces in a soda/lime batch. But the more of any of these colourants you add (some more than others of course), the more likely you're throwing off fit with your clear. But if you're not gathering over the colour or mixing it with clear or other colours in any way then have fun and experiment with increased concentrations of these colourants.
__________________
www.jmbglass.com
instagram.com/joshbernbaum_glass

Last edited by Josh Bernbaum; 09-17-2020 at 09:38 AM.
Reply With Quote
  #3  
Old 09-17-2020, 11:57 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,293
Pete VanderLaan is on a distinguished road
I'd be looking for some iron chromite and avoiding the hexavalent chromium scenario. Avoid reduction. I'll see what I can come up with in the formula library I have. It's not a color I ever make for myself. Copper and iron do make some lovely greens but only in a lead base.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #4  
Old 09-17-2020, 10:38 PM
Jacqueline Knight's Avatar
Jacqueline Knight Jacqueline Knight is offline
***
 
Join Date: Sep 2009
Location: Providence, RI
Posts: 141
Jacqueline Knight is on a distinguished road
Thank you Josh and Pete! I appreciate your input. We have been discussing melting half a bag of batch (10kgs) to test and see through a bit of trial and error. We have an 80kg colour pot furnace and want to melt some tests in the same atmosphere.

Interesting you ask about Gaffer batch re potassium or sodium. I can probably look up the MSDS. I like the idea of Manganese. Also just upping the Pot. Dichromate. We will just be blowing it straight and not trying to fit it with any other glass or colours so at least that is something we don't need to worry about.

Thank you for the note about the coffee grinder! And I look forward to any further information you can add, many thanks Pete
Reply With Quote
  #5  
Old 09-18-2020, 06:12 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,293
Pete VanderLaan is on a distinguished road
I am encouraging you to try to get away from the dichromate. It does produce hexavalent chromium which is well established as a carcinogen. Iron chromite would help with making the bottle green without those same issues. The great difficulty with chrome is its refractory nature and inability to be taken into solution. I have not been out to the studio to pursue recipes in the library but John Croucher and I were discussing this very issue a few months ago.
It would help to place any chromium compound you use in some lithium carbonate prior to the overall mix giving it a nice bath in some pretty aggressive stuff. I do that when making my dense black. These days, I use a juicer I got at a flea market. I got lots of them actually. They never last all that long.

I don't see why manganese would be helpful at all.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #6  
Old 09-20-2020, 04:46 AM
Peter Bowles Peter Bowles is offline
Registered User
 
Join Date: Sep 2002
Location: Breadalbane, Tasmania
Posts: 638
Peter Bowles is on a distinguished road
Talking

Hi Jacqueline, it looks like an Iron Chromate and Iron Oxide blend to me. I've got some samples from way back somewhere in the studio, I'll have a look in the next couple of days.
If you are serious about getting close to the tone and saturation there is a very useful system to use by casting a wedge shaped piece of glass from every sample you make. Firstly, it gives you a calculable colour density at any given thickness. And secondly (and even more usefully) it allows very quick tonal variations to be seen with variable thicknesses of two or more glasses.
Curious to know how much you will need to melt for your project?
Reply With Quote
  #7  
Old 10-11-2020, 11:25 PM
Jacqueline Knight's Avatar
Jacqueline Knight Jacqueline Knight is offline
***
 
Join Date: Sep 2009
Location: Providence, RI
Posts: 141
Jacqueline Knight is on a distinguished road
Hi Pete and Peter,

sorry for the delay in responding! Thank you so much for your replies and additional information. I would definitely heed your advice regarding the dichromate vs Iron Chromate. It is wonderful to get your opinions on this.
We do have a wedge mould for colour tests that we use. Initially we will melt small test batches, possibly 10 or 20kg melts to make sure we have the mix right, then we would melt an 80kg pot furnace. Our 400kg tank furnace is only used for clear.
Reply With Quote
  #8  
Old 10-12-2020, 09:22 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,293
Pete VanderLaan is on a distinguished road
Iron Chromate= Fe2(Cr04)3
Iron Chromite = Fe2(Cr04)
__________________
Where are we going and why am I in this basket?
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is Off
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 02:35 AM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2021, Jelsoft Enterprises Ltd.
© CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.