homemade unoxidized batch suggestions?

I'm interested in making an unoxidised batch, a 96, that has potassium, for melting sulfur/molybdenum ambers. Ive tried with our batch, East Bay regular, but the color doesn't take, I think because of the oxidizers. I know that SP sells a color base, and Im sure Jim would mix something for me but Id like to try myself.
I was going to start with Pete V's recipe of:
63.25 lbs sand
20.25 lbs soda ash
5.25 lbs potash
9.06 lbs hydrated lime
2.18 lbs 5 mole borax
Im considering upping the potash and decreasing the soda per and E&T's values but thought I'd see if any of you (perhaps Pete himself) had any suggestions.
Thanks in advance!
Reply With Quote
  #2  
Old 11-06-2019, 12:20 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,258
Pete VanderLaan is on a distinguished road
That's an old recipe of mine but it would work. I'd note that it lacks alumina which was a lot of my abandoning it.

It's slow to fine out without nitrates. Sulfur is not exactly a fun material to work with.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #3  
Old 11-06-2019, 05:23 PM
Kenny Pieper Kenny Pieper is offline
Registered User
 
Join Date: Feb 2003
Location: Burnsville N.C.
Posts: 844
Kenny Pieper is on a distinguished road
Paul my experience is that adding a small amount of zink makes this carbon amber more of a rich honey color. But too much and repeated cooling and heating will create a zink sulfide which is opaque and generally looks like shit. I add some sugar also for reduction and more carbon.
Reply With Quote
  #4  
Old 11-06-2019, 06:07 PM
Paul Stout Paul Stout is offline
Registered User
 
Join Date: Aug 2015
Location: Tucson AZ
Posts: 18
Paul Stout is on a distinguished road
Thanks Kenny, Ill make a note. Theres a bit of zinc oxide in the East Bays batch and I had wondered if that would adversely affect the color but I guess not, thanks for the tip
Reply With Quote
  #5  
Old 11-06-2019, 06:11 PM
Paul Stout Paul Stout is offline
Registered User
 
Join Date: Aug 2015
Location: Tucson AZ
Posts: 18
Paul Stout is on a distinguished road
Would adding black tin and sugar to East Bays batch create enough reduction to get the color to take, or do I just need to go ahead and make this unoxidised batch?
Reply With Quote
  #6  
Old 11-06-2019, 06:29 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,258
Pete VanderLaan is on a distinguished road
I never used this formula to make sulfur colors. It was promoted for copper rubies and silver glasses.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #7  
Old 11-06-2019, 07:47 PM
Josh Bernbaum Josh Bernbaum is offline
Registered User
 
Join Date: Feb 2009
Location: Brattleboro, VT
Posts: 722
Josh Bernbaum is on a distinguished road
If you have some of East Bay's regular batch to spare, why not do a test melt with it, 10 lbs. or something that's easily multipliable (is that a word?) And add the sulfur and sugar and black tin to that and see what happens. Or doesn't happen. Or how much it smells afterwards. A side note is that I've gotten some brown to amber tones on SP's oxidized batch by using quite a bit of manganese and a bit of iron. I think that's the manganese browning up on the all-sodium base which is SP.
__________________
www.jmbglass.com
instagram.com/joshbernbaum_glass
Reply With Quote
  #8  
Old 11-06-2019, 08:17 PM
Paul Stout Paul Stout is offline
Registered User
 
Join Date: Aug 2015
Location: Tucson AZ
Posts: 18
Paul Stout is on a distinguished road
I tried that without the black tin, just sulfur and sugar and it resulted in no color. I was going to try it with black tin, but Ive decided it would be better if I just make an unoxidised batch. Also a good learning project for me.
Reply With Quote
  #9  
Old 11-06-2019, 08:22 PM
Paul Stout Paul Stout is offline
Registered User
 
Join Date: Aug 2015
Location: Tucson AZ
Posts: 18
Paul Stout is on a distinguished road
Quote:
Originally Posted by Pete VanderLaan View Post
I never used this formula to make sulfur colors. It was promoted for copper rubies and silver glasses.
noted, thank you
Reply With Quote
  #10  
Old 11-07-2019, 08:47 AM
Ed Pennebaker's Avatar
Ed Pennebaker Ed Pennebaker is offline
Registered User
 
Join Date: Apr 2002
Location: Red Fern Glass in Clinton, Arkansas
Posts: 207
Ed Pennebaker is on a distinguished road
I usually found the carbon sulfur amber didn't need a fining agent. Maybe it produced enough bubbles to clear on its own? By the time it was up to 2350 there were just a few larger bubbles on the surface and didn't have any seeds. I thought is was one of the nicer colors to work with and easy to melt as a reducing color. I used powdered charcoal from a local charcoal plant (they dusted off their shelves to get powdered charcoal for me).
Reply With Quote
  #11  
Old 11-07-2019, 09:50 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,258
Pete VanderLaan is on a distinguished road
what you don't say Paul is how much sulfur you used on that first attempt. I recall making sulfur ambers using ordinary plate glass forty years back. I'm not clear at all that you need the absence of nitrates to do it. I would think that saltcake would give you some fining assistance if you tried it. I don't do it simply because the color is not to my taste. I would imagine that Helmer has lots of formulas for it.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #12  
Old 11-08-2019, 11:50 PM
Paul Stout Paul Stout is offline
Registered User
 
Join Date: Aug 2015
Location: Tucson AZ
Posts: 18
Paul Stout is on a distinguished road
Quote:
Originally Posted by Pete VanderLaan View Post
I never used this formula to make sulfur colors. It was promoted for copper rubies and silver glasses.
Quote:
Originally Posted by Pete VanderLaan View Post
what you don't say Paul is how much sulfur you used on that first attempt. I recall making sulfur ambers using ordinary plate glass forty years back. I'm not clear at all that you need the absence of nitrates to do it. I would think that saltcake would give you some fining assistance if you tried it. I don't do it simply because the color is not to my taste. I would imagine that Helmer has lots of formulas for it.
I used .04 percent sulfur in Jims Regular Batch and .005 percent sugar. I also added .09 percent soda ash. Too little perhaps?
Perhaps Ill try once more at .1 percent before moving on. Volf mentions potassium improving the color. I'll look into Helmer, and salt cake thank you for the suggestion.
Reply With Quote
  #13  
Old 11-09-2019, 11:14 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,258
Pete VanderLaan is on a distinguished road
If you are actually mixing my old clear formula, be careful not to confuse Calcium carbonate or whiting with hydrated lime. They yield totally different percentages of calcium oxide. The lime should be a type N and food grade is best.
Percentages of colorants are usually OK up to .1percent, not always. .04 is pretty light unless you have certain things you're trying to do. If you have "recipe Book" translated by Finn Lyngaard, it helps show fundamental formulations pretty well. Watch out for his typos. They're killers.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #14  
Old 11-10-2019, 05:34 PM
Greg Vriethoff's Avatar
Greg Vriethoff Greg Vriethoff is offline
Registered User
 
Join Date: Jan 2007
Location: Charlotte, NC
Posts: 2,244
Greg Vriethoff is on a distinguished road
Quote:
Originally Posted by Pete VanderLaan View Post
Sulfur is not exactly a fun material to work with.
I'm just trying to follow the logic here. I'm having a hard time seeing the sulfur in the formula posted. I assume it would be from the potash, but not all potash contains sulfur (correct?).

I know there's a lot I could be missing due to lack of experience.
__________________
Temperature and time.
Reply With Quote
  #15  
Old 11-10-2019, 05:51 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,258
Pete VanderLaan is on a distinguished road
The sulfur would be an additive to the basic mix. I'm suggesting that .1 percent would be a better place to start. I have also suggested elsewhere that if you use SP87 color base that it already contains a good deal of zinc so that adding more is not necessary. As it stands it could be a mismatch with SP87.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #16  
Old 11-11-2019, 11:19 AM
Josh Bernbaum Josh Bernbaum is offline
Registered User
 
Join Date: Feb 2009
Location: Brattleboro, VT
Posts: 722
Josh Bernbaum is on a distinguished road
It also could be noted here that the SP color base is (I suppose lower) expansion than the SP 87 oxidized since it leaves out the nitrates and antimony. When I had a phone call with Tom years ago I think I remember him mentioning adding 1.1 lbs. of soda to the 100 lbs. of unmixed color base to get expansion back to where the 87 oxidized is. I still haven't used any of the 1000 lbs. of his color base I have taking up precious space here though..
__________________
www.jmbglass.com
instagram.com/joshbernbaum_glass
Reply With Quote
  #17  
Old 11-11-2019, 12:01 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,258
Pete VanderLaan is on a distinguished road
Use Potash instead. It will help the color.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #18  
Old 12-26-2019, 11:16 PM
Paul Stout Paul Stout is offline
Registered User
 
Join Date: Aug 2015
Location: Tucson AZ
Posts: 18
Paul Stout is on a distinguished road
So quite a few melts later, I thought I'd go ahead and share my results.
a)I was melting too hot and turning the sulfur into sulfur dioxide which is just seedy clear
b)In East Bays regular batch I was able to get a nice amber by adding 1 percent sulfur and having the sugar be 1.25 times the amount of sulfur. In the attached picture the "columns" are all the same sulfur amount with increasing amounts of sugars in the "rows"
c)I was quite surprised that the sugar amounts made such a huge difference in the color.
d) large amounts of sugar (like two to three times the amount of sulfur) melted glasses that went fleshy opaque almost immedietaely when working, but the cullet was quite beautiful deep amber red with white agate looking streaks. Im thinking that the extra sugar allowed the sulfur to start to develop zinc sulfates in the glass (though I added no extra zinc, there is some in the batch)
e)this is the first color I've had to really work for and am really happy with it, though I still want to try it in a potash glass as suggested by Pete. Im also drawn towards the thought of adding some silver to see how it affects the color. . . any thoughts?
Thanks!

Last edited by Paul Stout; 12-26-2019 at 11:22 PM. Reason: grammatical corrections
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 12:21 PM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2021, Jelsoft Enterprises Ltd.
© CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.