Tool steel recommendations for cane chopper

I'm looking to build a cane chopper and was wondering what tool steel you guys would recommend for it? I found a post from David recommending A2, but he also got it further hardened. I don't know anyone around here that could harden it for me so ideally it would be something I can just buy online.
Reply With Quote
  #2  
Old 02-04-2018, 10:38 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 20,604
Pete VanderLaan is on a distinguished road
you might consider buying a set of replacement jaws for the Starrett nipper. I have yet to need to replace mine and they're over 25 years old.

Here's the actual tool and you can find the jaws in the parts section

http://www.starrett.com/metrology/pr...ail/1X-5%201~2
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #3  
Old 02-04-2018, 10:44 AM
Josh Bernbaum Josh Bernbaum is offline
Registered User
 
Join Date: Feb 2009
Location: Brattleboro, VT
Posts: 582
Josh Bernbaum is on a distinguished road
Old flat files were usually made with good quality tool steel in my experience.
You can cut them and grind the edges to two 45 degree angles. But good luck drilling holes in the stuff for mounting, however they can be welded in place on your chopper. I made one years ago out of an old arbor press.
__________________
www.jmbglass.com
instagram.com/joshbernbaum_glass
Reply With Quote
  #4  
Old 02-04-2018, 03:53 PM
Ben Solwitz Ben Solwitz is offline
Registered User
 
Join Date: May 2008
Location: Brooklyn, NY
Posts: 594
Ben Solwitz is on a distinguished road
I was hoping for something wider than the starrett jaws, would like to be able to cut a bunch of cane at once.
Reply With Quote
  #5  
Old 02-04-2018, 04:20 PM
Alex Stisser Alex Stisser is offline
Registered User
 
Join Date: Nov 2014
Location: western illinois
Posts: 10
Alex Stisser is on a distinguished road
old files are fine

Yes, keep it cheap and simple. Old curved or flat files are fine. Not quite as fancy as nice tool steel, but files are easy to find and a nice shape to hold and chop with. I've cut miles with this and it was made of scrap files and steel.
Attached Images
File Type: jpg IMG_4310.jpg (40.7 KB, 54 views)
File Type: jpg IMG_4311.jpg (40.6 KB, 50 views)
File Type: jpg IMG_4314.jpg (45.2 KB, 46 views)
Reply With Quote
  #6  
Old 02-04-2018, 04:50 PM
Ben Solwitz Ben Solwitz is offline
Registered User
 
Join Date: May 2008
Location: Brooklyn, NY
Posts: 594
Ben Solwitz is on a distinguished road
I found a previous thread where Wes recommended tungsten carbide like this:
https://centennialcarbide.com/flat-blanks/

Would I totally ruin a diamond blade if I cut one of those blanks with it?
Reply With Quote
  #7  
Old 02-05-2018, 09:12 AM
Kenny Pieper Kenny Pieper is offline
Registered User
 
Join Date: Feb 2003
Location: Burnsville N.C.
Posts: 818
Kenny Pieper is on a distinguished road
I made a cane chopper years ago and used a file for the blades. If you heat the file up to a cherry red with a torch and let it cool slowly it will soften it so that you can easily cut, grind, and drill it. Then to harden it heat it back up to a cherry red and quince it in old motor oil (water will work but not as well) and then temper it by putting it in a oven at around 400f for 20 min. The blades will last a decade.
Reply With Quote
  #8  
Old 02-05-2018, 11:41 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 20,604
Pete VanderLaan is on a distinguished road
Quote:
Originally Posted by Kenny Pieper View Post
Then to harden it heat it back up to a cherry red and quince it in old motor oil (water will work but not as well) and then temper it by putting it in a oven at around 400f for 20 min..
********
Ignorance display time:

Why does this work?
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #9  
Old 02-05-2018, 01:27 PM
Carlos Reckner Carlos Reckner is offline
Registered User
 
Join Date: Jul 2012
Location: Near Bethlehem, PA
Posts: 22
Carlos Reckner is on a distinguished road
Slow cooling allows the carbon in the steel to diffuse making the part "soft". Heating and quenching locks the carbon in the crystal structure of the steel. Look up Martensite or martensitic transformation. After quenching the steel will have a lot of stress and be hard but brittle. Tempering draws the hardness down some, but relieves some of the stress giving the part toughness.
This is why the average hardware material does not harden well, or at all. Not enough carbon in the mix.
If I remember correctly files were oil hardening. There are steels that are water hardening as well as air hardening. Just depends on the recipe for the steel.
Reply With Quote
  #10  
Old 02-05-2018, 03:41 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 20,604
Pete VanderLaan is on a distinguished road
When I was visiting Scott Benefield in Belfast, we spent an evening being slowly intoxicated by a tv show on carbon in steel. Then I watched Forged in Fire on cable and those guys would quench and the whispering golf pro types would say "God, he's quenching again!!"

Then the guy in Pennsylvania burned down his entire neighborhood.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #11  
Old 02-05-2018, 06:50 PM
Rich Samuel's Avatar
Rich Samuel Rich Samuel is offline
Registered User
 
Join Date: Apr 2002
Location: Seattle, WA
Posts: 2,402
Rich Samuel is on a distinguished road
Guy in NY, that is. Cohoes, NY.

https://www.bizjournals.com/albany/n...-loans-to.html
Reply With Quote
  #12  
Old 02-14-2018, 09:06 PM
Steve Beckwith Steve Beckwith is offline
Registered User
 
Join Date: Feb 2007
Location: Cocoa Beach, Florida
Posts: 87
Steve Beckwith is on a distinguished road
Not all files are suitable to make tools like this. From what I understand, modern files made on Mexico are low grade steel with chemical case hardening on the exterior. Older files, made in USA are generally good tool steel.
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is Off
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 06:29 AM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2019, Jelsoft Enterprises Ltd.
CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.