  #1  
Old 12-05-2019, 03:47 PM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 460
Shawn Everette is on a distinguished road
uv delamination

Hey ya'll. So I'm trying to help out my partner on a restoration project at a museum. She's got an assembled cut and polished piece that is starting to get the tell tale delam ferns growing at the seams. There's an odd oil slick look to part of it, which I haven't come across before. We think that it was bonded with a UV, which I know is not our favorite. Anybody have experience on how long to expect complete failure?
Attached Images
File Type: jpg CON_2018.239_nt_001.jpg (15.3 KB, 59 views)
File Type: jpg CON_2018.239_nt_003.jpg (21.5 KB, 55 views)
File Type: jpg CON_2018.239_nt_005.jpg (32.8 KB, 56 views)
Reply With Quote
  #2  
Old 12-05-2019, 04:14 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,582
Pete VanderLaan is on a distinguished road
Complete failure? It probably won't but it will continue to look worse and worse. The "artifact" or the fern is the result of inadequate exposure to the UV source. The ring may well indicate how flat the two surfaces were at the time of joining them. Newton rings sugggest very close fits.
During the period when I was trying to use UV before abandoning it was that the light source needs to be warmed up. We finallly kept our light under a cardboard box running all day. If you don't warm them up, the filament develops a coating that interfers with the bonding.

I've taken them apart using Methyl Chloride ( Toxic) but it's a lot faster to bite the bullet and saw them, resurfacing everything and this time doing it in Hxtal.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #3  
Old 12-05-2019, 04:44 PM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 460
Shawn Everette is on a distinguished road
Any chance you could manage to properly cure what hasn't started to come apart. Given the dogma of museum conservation disassembly probably isn't happening, certainly not with a saw.
Reply With Quote
  #4  
Old 12-05-2019, 06:30 PM
Larry Cazes Larry Cazes is offline
Registered User
 
Join Date: Feb 2006
Location: San Jose, CA
Posts: 950
Larry Cazes is on a distinguished road
Quote:
Originally Posted by Shawn Everette View Post
Anybody have experience on how long to expect complete failure?
Exactly 1 year 3 months and 10 hours. Thats give or take a few seconds of course.
Reply With Quote
  #5  
Old 12-05-2019, 06:59 PM
Jordan Kube Jordan Kube is online now
?
 
Join Date: Aug 2003
Location: Seattle, WA
Posts: 1,702
Jordan Kube is on a distinguished road
Quote:
Originally Posted by Shawn Everette View Post
Any chance you could manage to properly cure what hasn't started to come apart.
My gut feeling says no but that's the easiest place to start. Won't cost anything. If it doesn't work you're still at present condition.

I know it's not your problem but I would recommend they contact the artist and try to work out a remedy. Museums should have museum quality work, which this piece is not at this point. If the artist isn't interested(I'm assuming they are still around) stick it in a box in back and let it fall apart out of public view.
__________________
WWUD? Think for yourself.
Reply With Quote
  #6  
Old 12-05-2019, 10:23 PM
Scott Dunahee's Avatar
Scott Dunahee Scott Dunahee is offline
Registered User
 
Join Date: Apr 2002
Location: Madison, WI
Posts: 638
Scott Dunahee is on a distinguished road
can't you bring it up to temp and burn out the uv glue connections then reassemble after cleaning with hxtal?

Just asking.

BSD
__________________
That's all right. I never expected there to be a blue light special on enlightenment...
Reply With Quote
  #7  
Old 12-06-2019, 12:23 AM
David Patchen's Avatar
David Patchen David Patchen is offline
Registered User
 
Join Date: Sep 2005
Location: San Francisco, CA
Posts: 1,902
David Patchen is on a distinguished road
Quote:
Originally Posted by Scott Dunahee View Post
can't you bring it up to temp and burn out the uv glue connections then reassemble after cleaning with hxtal?
BSD
This is what the artist should do. If he won't, this is what I would do. I've taken pieces off of bases by bringing them up and down through another annealing cycle. The UV turns dark brown and fails. It isn't easy to get off but a super clean razor blade and some acetone should do the trick. Maybe a cork belt and cerium if it's really stubborn. Then re-assemble with hxtal.
Reply With Quote
  #8  
Old 12-06-2019, 01:23 AM
Steven O'Day Steven O'Day is offline
Registered User
 
Join Date: Jun 2002
Location: portland oregon
Posts: 319
Steven O'Day is on a distinguished road
Buy a new one?

https://nestcasa.com/product/herkimer-candleholder/
Reply With Quote
  #9  
Old 12-06-2019, 07:47 AM
Monte Becker Monte Becker is offline
Registered User
 
Join Date: Jan 2017
Location: Massachusetts
Posts: 13
Monte Becker is on a distinguished road
low cost but fail again?

Quote:
Originally Posted by Steven O'Day View Post
Shoot - that's a whole lot less expensive then taking it apart and fixing it - and it's 10% off... But, there's no saying it won't fail the same way...
Reply With Quote
  #10  
Old 12-06-2019, 08:38 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,582
Pete VanderLaan is on a distinguished road
It will completely delaminate in an oven at 300F. You just bonk it apart with a mallet. I takes a fair amount if clean up.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #11  
Old 12-06-2019, 09:30 AM
Tom Fuhrman Tom Fuhrman is offline
Registered User
 
Join Date: Apr 2002
Location: hills of Tennessee
Posts: 1,432
Tom Fuhrman is on a distinguished road
I've seen some very early pieces made in the early 70s that were silicone together and were in some prominent museums that were failing. The question then arises, do they get repaired and put back together with the original materials or are they reassembled using newer adhesives. Museum restorations can be a very sticky wicket. One in particular that I recall was a stacked assemblage of mirrored glass balls.
Reply With Quote
  #12  
Old 12-06-2019, 09:54 AM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 460
Shawn Everette is on a distinguished road
So this is the on the money point. I know how to take it apart and reglue it, it's just against nearly all modern conservation protocol to do that. There's a weird dichotomy in their world, one allows full invasive restoration, the other is only preventative maintenance. We're dealing with the latter.

After talking about it they're probably going to just add some hxtal in enough places to keep it together. I believe that this may be one of their "design" pieces, so there is no artist to shove it back on.

Steven's post is by far my favorite.
Reply With Quote
  #13  
Old 12-06-2019, 10:30 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,582
Pete VanderLaan is on a distinguished road
It will only come apart if you put it up over your bed and try to sleep under it.

Don't get me started on the advantages the world would have if it crashed catastrophically to a hard concrete floor. Crocodile tears would fall.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #14  
Old 12-06-2019, 10:52 AM
John Riepma John Riepma is offline
Registered User
 
Join Date: Apr 2003
Location: Grand Haven, MI
Posts: 509
John Riepma is on a distinguished road
Or the museum could do what Damien Hirst did when the shark "preserved" in formaldehyde that he sold for $11,000,000 starting rotting in the tank of formaldehyde. I had heard that initially when the collector wanted it conserved he convinced them that the deterioration was part of the process. Eventually the shark was replaced with a "new" (albeit still dead) shark.

https://www.dailyartmagazine.com/sto...n-hirst-shark/

This has always amazed me, the amounts of money that insecure billionaires will spend to have something no one else can have. I just wish I was good enough to make a story like this up.
Reply With Quote
  #15  
Old 12-06-2019, 11:03 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,582
Pete VanderLaan is on a distinguished road
I could send you a dead chicken if you like. Cast in resin?
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #16  
Old 12-06-2019, 01:40 PM
John Riepma John Riepma is offline
Registered User
 
Join Date: Apr 2003
Location: Grand Haven, MI
Posts: 509
John Riepma is on a distinguished road
I'd prefer an endangered species. More "arty", y'know. Then I'd just have to write some long-winded artist statement and suppress my morals ling enough to put the appropriate number of zeros and commas on the price tag. and probably change my wardrobe to include a beret and ascot and what-all else the successful artists are wearing these days.
Reply With Quote
  #17  
Old 12-06-2019, 03:56 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,582
Pete VanderLaan is on a distinguished road
Just be careful with your use of the negative space..
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #18  
Old 12-07-2019, 07:45 AM
Brian Wong Shui Brian Wong Shui is offline
Registered User
 
Join Date: Oct 2002
Location: Atlanta, GA
Posts: 176
Brian Wong Shui is on a distinguished road
Wonder what the conservators would do about this?

https://www.cbsnews.com/news/art-bas...ch-2019-12-06/
Reply With Quote
  #19  
Old 12-07-2019, 10:35 AM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 460
Shawn Everette is on a distinguished road
Have a stroke.
Reply With Quote
  #20  
Old 12-08-2019, 06:06 PM
Rick Wilton Rick Wilton is offline
Registered User
 
Join Date: Oct 2005
Location: Calgary, Alberta Canada
Posts: 207
Rick Wilton is on a distinguished road
If it'll fit in a microwave that works well for me taking glass awards apart. The glue gets heated by the microwaves 3 minutes is usually enough.
Reply With Quote
  #21  
Old 12-09-2019, 08:24 PM
Michael Ahlefeldt-Laurvig Michael Ahlefeldt-Laurvig is offline
Registered User
 
Join Date: Apr 2010
Location: Sweden
Posts: 766
Michael Ahlefeldt-Laurvig is on a distinguished road
Steven,
Did you picture google in some way to find it?
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is Off
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 03:55 PM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2020, Jelsoft Enterprises Ltd.
CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.