CraftWEB Hot Glass Talk  

Go Back   CraftWEB Hot Glass Talk > Hot Glass > Antiques & Classics

Reply
 
Thread Tools Display Modes
  #1  
Old 06-30-2002, 12:58 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,495
Pete VanderLaan is on a distinguished road
Photos of the Portland Furnaces.

This is the element protruding thru a soft brick. The shank is 7/16th inch diameter and fifteen inches long.. The outer two inches is the connection section for the electric strap. The next nine inches is in the brick and then it enters the crown. the very last half inch of the shank has to be inside of the furnace.. The thinner port, which isn't in this picture is the heating portion. Jons was 18 inch, Steve's was 12 inch.
Attached Images
File Type: jpg furn18.jpg (12.6 KB, 1782 views)
Reply With Quote
  #2  
Old 06-30-2002, 01:04 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,495
Pete VanderLaan is on a distinguished road
These are the elements entering Steves' crown. The straps are bringing the power from the transformer. You can get either stainless steel or aluminum straps. The aluminum ones come with the elements at no extra charge. I got the stainless ones. They have to be tight.( torque them down)
Note the plastic tubes that are pumping air at the connectors. Cool connectors are happy connectors. Good idea Steve.
Attached Images
File Type: jpg full shot of element.jpg (18.7 KB, 1679 views)
Reply With Quote
  #3  
Old 06-30-2002, 01:12 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,495
Pete VanderLaan is on a distinguished road
This is a shot of the full element ( almost) going thru the brick. Note on the left where it has gotten thinner. Thats the business end. The hand is Steves'.
Attached Images
File Type: jpg full shot of the element.jpg (14.0 KB, 1608 views)
Reply With Quote
  #4  
Old 06-30-2002, 05:32 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,495
Pete VanderLaan is on a distinguished road
This is a sideways shot of the transformer with the cover off. We'll have to wait til my daughter gets home to rotate it. These are seriously heavy little buggers. This one was about 2x2x3 feet and weighed about 600 lbs. Used they can cost whatever you can pay, as little as $200 dollars. New its a 1500 dollar item. Hard to re-sell at garage sales.
Attached Images
File Type: jpg furn16.jpg (28.1 KB, 1608 views)
Reply With Quote
  #5  
Old 06-30-2002, 05:40 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,495
Pete VanderLaan is on a distinguished road
This is Jons' transformer in place. Note how it is much cleaner than Steves was. Note that it cost much more since it was new. Both work fine.
Attached Images
File Type: jpg furn10.jpg (21.6 KB, 1575 views)
Reply With Quote
  #6  
Old 06-30-2002, 05:43 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,495
Pete VanderLaan is on a distinguished road
This is Jon's transformer next to the panel that contains the silicon Controlled rectifier ( SCR) It gives you an idea of how much space this junk actually takes up. ( not much)
Attached Images
File Type: jpg furn7.jpg (17.8 KB, 1539 views)
Reply With Quote
  #7  
Old 06-30-2002, 05:53 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,495
Pete VanderLaan is on a distinguished road
Here is the Watlow 150 AMP SCR on its side. I have no idea what I will do when the kids leave home.
Attached Images
File Type: jpg furn6.jpg (19.6 KB, 1528 views)
Reply With Quote
  #8  
Old 06-30-2002, 05:56 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,495
Pete VanderLaan is on a distinguished road
This is the relay which controls the on/off function from the controller to the SCR.
Attached Images
File Type: jpg furn5.jpg (23.0 KB, 1481 views)
Reply With Quote
  #9  
Old 06-30-2002, 06:00 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,495
Pete VanderLaan is on a distinguished road
This is a shot of the top of Jons' furnace. Everyone is supposed to gasp at the exposed fiber. I preferred to gasp at how easy it was to stick your hand in there and get killed by the exposed connectors. It has a cover and it should have been in place. I'll bet the farm that it isn't in place right now. This is seriously dangerous.
You can see the straps going from element to element. Jons furnace had six eighteen inch ones. He never really turns it up high which I though he should do for the visiting clowns. He didn't.
Attached Images
File Type: jpg furn4.jpg (22.5 KB, 1529 views)
Reply With Quote
  #10  
Old 06-30-2002, 06:04 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,495
Pete VanderLaan is on a distinguished road
This is a shot of the door "kill" switch. ( What an appropriate name). It doesn't show well but it is a little momentary switch from Graingers that opens the circuit when you swing the door open. I didn't like their doors. If they had fit better you would not have known that these furnaces were on and were melting batch. It was very strange.
Attached Images
File Type: jpg furn3.jpg (20.3 KB, 1498 views)
Reply With Quote
  #11  
Old 06-30-2002, 06:07 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,495
Pete VanderLaan is on a distinguished road
This really shows what the connector straps and the element tops look like.
Attached Images
File Type: jpg furn1.jpg (20.9 KB, 1470 views)
Reply With Quote
  #12  
Old 02-07-2003, 03:16 PM
Dan Buchacher Dan Buchacher is offline
Registered User
 
Join Date: Apr 2002
Location: Seattle
Posts: 189
Dan Buchacher is on a distinguished road
Is it intended that these element units complete with supporting soft bricks are easily removed like a plug, and replaced when they fail?

Do these elements extend down around the sides of the crucible or is this all top fired?
__________________
Dan
Reply With Quote
  #13  
Old 02-07-2003, 04:53 PM
Bryan Harnois
Guest
 
Posts: n/a
design questions...Jon,Steve,Pete

I've been looking at these pictures again recently and a few questions also came to mind of the makers of this design..Jon, Steve and now Pete

From the posted pics and text from Pete we have the following dimensions -
the thicker connecting shank is 15" long, 2" at top of the brick for connections, 9" in the brick, leaving 4" protruding from the brick on the furnace side, the last 1/2" of whick needs to be inside the furnace

So. how thick are we casting these crowns, of what castable, and are the holes in the crown and the soft bricks tapered or not? Are these flat crowns or slightly domed?

The dimensions posted above would indicate that at least 3" of the shank portion of the element are sitting in a small ' well ' in the castable...is this the most healthy configuration for the shank area...would it be better if just the required last 1/2" of the shank was exposed to the heat of the chamber?

Further, if Pete looks at this, what castable did you finally decide on for the floor and main heating chamber of the new furnace, and did you go with the front of the heating chamber and gathering port being detachable from the rest for cleanout and pot changes as you have described for your gas furnaces?

Lots of questions, but I'm hoping to start my 150# furnace once the frigid weather warms up here on the edge of the North Atlantic

thanks

Bryan
Reply With Quote
  #14  
Old 02-07-2003, 08:03 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,495
Pete VanderLaan is on a distinguished road
This does presume a three inch thick crown and I do think thicker might be better, by one inch. Mass is important in electric furnaces although it is a tradeoff with strength. The brick does just sit in the well.

My castable will be Morocast 99 % alumina. II was really impressed with the Morocast 95 and Tom suggested I try this stuff too. I will be using 18 inch by eighteen inch by one inch paver tile from Engineered ceramics as well.

This furnace will open from the side with a giant refrigerator door to remove the pots.
Reply With Quote
  #15  
Old 02-07-2003, 09:58 PM
Bryan Harnois
Guest
 
Posts: n/a
paver tile

and the paver tile goes....where?

Bryan
Reply With Quote
  #16  
Old 02-18-2004, 04:42 PM
Durk Valkema
Guest
 
Posts: n/a
Moly

"Note the plastic tubes that are pumping air at the connectors. Cool connectors are happy connectors. Good idea"
Sure but the air is their to keep the crappy fumes inside the furnace from condensating on your elements lead-through the bricks.
Element failure in no time for sure.
Been building these furnaces since the 80th, with the expensive kanthal elements, one thing, they did publish excellent guidebooks.
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is On
Forum Jump


All times are GMT -5. The time now is 12:20 AM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2019, Jelsoft Enterprises Ltd.
© CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.