Moly element failure

We are going through a crucible change for our 400# Stadelman furnace and finished and turned on the furnace and it started to spark from this element. It is a new element with a new strap. At first it broke off right at the line between the light gray and dark gray of the element. After taking off the top piece that broke away, we tried to attach the straps to just the remaining dark gray length. Turned it on and continued to get more sparks. Unfortunately, this was the 3rd element that we replaced today, and our last spare.
We have another older one that we replaced because it broke off on the same line that we will try and put back in service...
Any ideas why this may be happening???
Attached Images
File Type: jpg Broken element.jpg (34.1 KB, 49 views)
Reply With Quote
  #2  
Old 09-06-2019, 05:32 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,933
Pete VanderLaan is on a distinguished road
It sounds like it was cracked in more than one place.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #3  
Old 09-06-2019, 06:29 PM
Mark Rosenbaum's Avatar
Mark Rosenbaum Mark Rosenbaum is offline
Registered User
 
Join Date: Apr 2002
Location: New Orleans, LA
Posts: 1,061
Mark Rosenbaum is on a distinguished road
Quote:
Originally Posted by Pete VanderLaan View Post
It sounds like it was cracked in more than one place.
I guess... it tested out, but when we turned on the juice, kaPOW!!!!
Reply With Quote
  #4  
Old 09-06-2019, 08:19 PM
Brian Wong Shui Brian Wong Shui is online now
Registered User
 
Join Date: Oct 2002
Location: Atlanta, GA
Posts: 179
Brian Wong Shui is on a distinguished road
Maybe some twisting going on while the straps were being tightened or maybe over tightening the strap (ie crushing the shank and causing cracks).
Reply With Quote
  #5  
Old 09-07-2019, 08:17 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,933
Pete VanderLaan is on a distinguished road
When I've seen this happen, it invariably comes from an overtightening of the strap. In testing , the crushed material still conducts and shows continuity but once power is applied it expands rapidly and shows the failure. I have so far not seen one do it in two places but it's the likely explanation.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #6  
Old 09-08-2019, 10:19 PM
Scott Novota's Avatar
Scott Novota Scott Novota is offline
AbbyNormal User
 
Join Date: Jan 2004
Location: Pensacola Florida
Posts: 2,160
Scott Novota is on a distinguished road
Ah man this is really a hard blow. I sympathize.

I have two spare elements at the shop but I am almost positive they are the size smaller than you use. If however, they are the same size I am happy to help. They are the smaller of the two that Steve pushed out the door and where on Ardin's furnace. Give me a call if you think might need one.
Reply With Quote
  #7  
Old 09-09-2019, 06:32 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,933
Pete VanderLaan is on a distinguished road
you can install the 9/18 312/500 as a replacement but you have to put one in each bank to balance it. It will lose wattage but will work.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #8  
Old 09-09-2019, 10:14 AM
Mark Rosenbaum's Avatar
Mark Rosenbaum Mark Rosenbaum is offline
Registered User
 
Join Date: Apr 2002
Location: New Orleans, LA
Posts: 1,061
Mark Rosenbaum is on a distinguished road
Quote:
Originally Posted by Scott Novota View Post
Ah man this is really a hard blow. I sympathize.

I have two spare elements at the shop but I am almost positive they are the size smaller than you use. If however, they are the same size I am happy to help. They are the smaller of the two that Steve pushed out the door and where on Ardin's furnace. Give me a call if you think might need one.
I appreciate it Scott! I think that those are smaller because Arden's (yours) is a smaller furnace.... We are going to Orange Beach this weekend. Are you going to be around?
Reply With Quote
  #9  
Old 09-09-2019, 10:16 AM
Mark Rosenbaum's Avatar
Mark Rosenbaum Mark Rosenbaum is offline
Registered User
 
Join Date: Apr 2002
Location: New Orleans, LA
Posts: 1,061
Mark Rosenbaum is on a distinguished road
Quote:
Originally Posted by Pete VanderLaan View Post
you can install the 9/18 312/500 as a replacement but you have to put one in each bank to balance it. It will lose wattage but will work.
I am getting Cheyenne's last two elements. Those will be spares. He is ordering more because there is now a "need", so I will stock up again until I have enough for a full change. You have to have back-ups for consumables... a friend always tells me that
Reply With Quote
  #10  
Old 09-09-2019, 02:54 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,933
Pete VanderLaan is on a distinguished road
The 300# takes a 9/18 312/500
The 28 inch ( about 430#) takes the 9/18 450/500 ( or..550)

Without looking in the big book of numbers, the smaller set uses about 1500 less watts. You can always include a balanced pair of elements in a pinch but they have to be balanced to the banks.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #11  
Old 09-09-2019, 09:04 PM
Scott Novota's Avatar
Scott Novota Scott Novota is offline
AbbyNormal User
 
Join Date: Jan 2004
Location: Pensacola Florida
Posts: 2,160
Scott Novota is on a distinguished road
Oh yes...I will be around for sure. Let me know what your plans are and when you will be free and we can line something up. We can figure out what works. Here, there, whatever.

If you don't still have my number let me know.

Last edited by Scott Novota; 09-09-2019 at 09:06 PM.
Reply With Quote
  #12  
Old 09-10-2019, 07:38 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,933
Pete VanderLaan is on a distinguished road
Quote:
Originally Posted by Mark Rosenbaum View Post
I am getting Cheyenne's last two elements. Those will be spares. He is ordering more because there is now a "need", so I will stock up again until I have enough for a full change. You have to have back-ups for consumables... a friend always tells me that
****
When I was doing elements a cardinal rule around here was to never ship them twice. Tweaking the nose of Buddah comes up. I'm surprised that he's doing it that way but it's good for you.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #13  
Old 09-10-2019, 10:40 AM
Mark Rosenbaum's Avatar
Mark Rosenbaum Mark Rosenbaum is offline
Registered User
 
Join Date: Apr 2002
Location: New Orleans, LA
Posts: 1,061
Mark Rosenbaum is on a distinguished road
Quote:
Originally Posted by Scott Novota View Post
Oh yes...I will be around for sure. Let me know what your plans are and when you will be free and we can line something up. We can figure out what works. Here, there, whatever.

If you don't still have my number let me know.
I don't have your #... do you have mine? Text me yours if you do.
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is Off
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 09:53 AM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2020, Jelsoft Enterprises Ltd.
CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.