Glass on floor of my pottery kiln

Hi guys,

I use my wife’s pottery kiln with a computerized controller as my annealer. She still uses it for pottery. She fired a load (2350 F) the other day and did not vacuum it out well beforehand and left a broken piece of glass in the bottom. It has melted abound a quarter inch deep into the soft fire brick on the floor of the kiln.

Do I need to get in there and dig it out before she fires it up high ago? Will it eventually melt all the way through if I don’t? I assume I do, I just thought I would check with y’all first.

Thanks for your feedback!
__________________
_________________________________________
Growing old is mandatory. Growing up is optional!
Reply With Quote
  #2  
Old 11-08-2017, 10:36 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 20,956
Pete VanderLaan is on a distinguished road
If it's removed easily, remove it.
If not, the tendency is that as the glass interacts with the fireclay, it gets progressively more and more non glasslike and pretty much stops dissolving things. It will eventually turn opaque as the fireclay dominates more and more. .
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #3  
Old 11-08-2017, 12:14 PM
Steven O'Day Steven O'Day is offline
Registered User
 
Join Date: Jun 2002
Location: portland oregon
Posts: 305
Steven O'Day is on a distinguished road
If the floor is insulating brick it will dissolve the brick and stop, this will be deeper than with firebrick. In our school kilns I usually remove it if it is still a shiny blob and let it sit if it has sunk in.
Reply With Quote
  #4  
Old 11-08-2017, 01:51 PM
Greg Vriethoff's Avatar
Greg Vriethoff Greg Vriethoff is offline
PotatoFish
 
Join Date: Jan 2007
Location: Charlotte, NC
Posts: 2,042
Greg Vriethoff is on a distinguished road
Don't worry, it's like xenomorph blood. It'll slow down after a few levels before it breeches the hull.

Seriously, what Pete said. If it's been taken up to 2350 already I don't think it's going to move much more.
__________________
"Technique is just a means of arriving at a statement." - Jackson Pollack
Reply With Quote
  #5  
Old 11-08-2017, 09:04 PM
David Balkon David Balkon is offline
Registered User
 
Join Date: Jan 2013
Location: Nashville, TN
Posts: 30
David Balkon is on a distinguished road
Thanks for the feedback.
__________________
_________________________________________
Growing old is mandatory. Growing up is optional!
Reply With Quote
  #6  
Old 11-10-2017, 01:58 PM
Franklin Sankar's Avatar
Franklin Sankar Franklin Sankar is offline
Registered User
 
Join Date: Apr 2002
Location: Trinidad, West Indies
Posts: 3,817
Franklin Sankar is on a distinguished road
That is the best news. My floor is a mess
Franklin
Reply With Quote
  #7  
Old 11-10-2017, 04:09 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 20,956
Pete VanderLaan is on a distinguished road
Quote:
Originally Posted by Franklin Sankar View Post
That is the best news. My floor is a mess
Franklin
******
Don't go getting cocky.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #8  
Old 11-10-2017, 05:18 PM
Franklin Sankar's Avatar
Franklin Sankar Franklin Sankar is offline
Registered User
 
Join Date: Apr 2002
Location: Trinidad, West Indies
Posts: 3,817
Franklin Sankar is on a distinguished road
Sorry Lesson learnt but too late. It will be interesting to see what happens. Floor has a layer of expired refractory cement and sand.
Franklin
Reply With Quote
  #9  
Old 11-15-2017, 03:59 PM
Scott Novota's Avatar
Scott Novota Scott Novota is offline
AbbyNormal User
 
Join Date: Jan 2004
Location: Pensacola Florida
Posts: 2,140
Scott Novota is on a distinguished road
I have been known to fill them with brick mortar after they stop dissolving the IFB like cotton candy someone spit on.

Not that the inside of my glory hole is pock marked with such things...no sir!
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is Off
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 08:18 AM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2019, Jelsoft Enterprises Ltd.
© CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.