Lino's Nero Tea

That's what we called it at Manifesto anyway.

Sand 100
Soda 44
Calcium 16
Boric Acid 3
Sulphur 3.950
Rosin 1.3
Iron Oxide 2.850
Black Nickle Oxide 1

Just for cane or threading. Overlay onto gaffer duro white for extra opaqueness in those super stretched out cane pick ups. Fun to melt. Not as bad as Pete would have you believe

Have fun kids.
__________________
WWUD? Think for yourself.
Reply With Quote
 


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 05:55 PM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2020, Jelsoft Enterprises Ltd.
CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.