fenton red bubbles

We melt fenton red cullet on occasion. It is a cad/sel red. It was a casting glass for them. When I melt it I have always had to squeeze it and leave it around 2040 F or else we end up with lots of large bubbles( reboil is what I've heard this is called.) I would like to hold it at a higher temp than that. As well as I would like to know whats going on with the bubbles and where are they coming from. It doesn't seem like they will just rise out and go away. Thanks
Reply With Quote
  #2  
Old 10-14-2017, 08:18 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 19,822
Pete VanderLaan is on a distinguished road
Sulfide Gas, and everyone who melts this stuff has the same issues. Get it too cold and it will switch valence, make tiny bubbles and change color.
Kenny always called them "Smokers".
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #3  
Old 10-14-2017, 12:47 PM
Shawn Watt Shawn Watt is offline
Registered User
 
Join Date: May 2010
Location: Branson, MO
Posts: 96
Shawn Watt is on a distinguished road
Is there higher temperature range that it would change valence and reabsorb the sulfide gas? Im at 2040 now and it just a bit slow
Reply With Quote
  #4  
Old 10-14-2017, 01:00 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 19,822
Pete VanderLaan is on a distinguished road
No. The trouble with cad sel reds is the sulfur. Cadmium is colorless in glass without the sulfur. Remember it's a cadmium-sulfo selenium glass. It has to have all three and one is a pure sociopath. There's more of it than you need in Cadmium sulfide and it really is better made with some of the cad sulfide and some cad oxide to get the cadmium level right but it usually isn't done that way. As Chuck Savoie used to say, "sulfur is not your friend in a red glass.". Taking the glass down in temperature does help but obviously makes it more viscous. Go too far and the valence switches and it turns brown. It's not a cooperative glass and even worse if you are having to use someone else's cullet. I picked bubbles from mine in large pieces.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #5  
Old 10-15-2017, 01:19 PM
Shawn Watt Shawn Watt is offline
Registered User
 
Join Date: May 2010
Location: Branson, MO
Posts: 96
Shawn Watt is on a distinguished road
Thanks for the info Pete
Reply With Quote
  #6  
Old 10-19-2017, 12:59 PM
Jordan Kube Jordan Kube is offline
?
 
Join Date: Aug 2003
Location: Seattle, WA
Posts: 1,572
Jordan Kube is on a distinguished road
Some of the boro guys are using encapsulated cadmium and getting great results. No off gassing, nice colors, and added to cullet.
__________________
WWUD? Think for yourself.
Reply With Quote
  #7  
Old 10-19-2017, 03:15 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 19,822
Pete VanderLaan is on a distinguished road
seems to me that encapsulated is a fancy term for such things as Cadmium selenate which is a compound. We did use it back when Chuck and I were doing the color rods but the difference wasn't really appreciable. The goal needs to be getting the sulfur content down to where it should be. Cad sulfide just has way more than you need. I would agree that the boro guys are getting good results . I suspect it's since the boro is so much more viscous than a zinc potash glass would be at a fixed temp. I think the other aspect of using the compounds is there is less volatilization. I haven't seen anyone really prove that out.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #8  
Old 10-19-2017, 04:02 PM
Jordan Kube Jordan Kube is offline
?
 
Join Date: Aug 2003
Location: Seattle, WA
Posts: 1,572
Jordan Kube is on a distinguished road
No, it is zirconium silica encapsulation. Cool stuff.

Overview:
https://www.highwaterclays.com/index...ted-stains.cfm

Fun stuff: click download to see full text
https://www.researchgate.net/profile...ed-Pigment.pdf

My friend remelted some cadmium yellow from Northstar and experienced the smoking and off gassing one might expect. He mixed his own using the encapsulated cadmium and didn't get any off gassing. It was a really nice yellow too. He added some holmium and got a little bit of a red shift in the UV range. I'm not sure which manufacturer he is using.

It would be interesting to investigate in soft glass.
__________________
WWUD? Think for yourself.

Last edited by Jordan Kube; 10-19-2017 at 04:05 PM.
Reply With Quote
  #9  
Old 10-19-2017, 05:35 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 19,822
Pete VanderLaan is on a distinguished road
When I've looked at the recent stuff, it's pretty closed tech. I've seen zinc, sodium and barium based stuff but not zircon at this point. Get after it.
__________________
Where are we going and why am I in this basket?
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 05:11 AM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2018, Jelsoft Enterprises Ltd.
© CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.