Hxtal

Iíve been playing with glueing on bases... any advice on glueing to stainless or granite/quartz? Does it hold up? Seems to be working so far but always hard to sleep under.
Reply With Quote
  #2  
Old 07-17-2019, 07:48 AM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 510
Shawn Everette is on a distinguished road
Honestly you should be gtg on granite or quartz in the majority of cases. As long as there's no type of clear coat that's a pretty excellent surface to bond to. The main enemy of hxtal is going to be plastic or flexible surfaces.
Reply With Quote
  #3  
Old 07-17-2019, 09:08 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,690
Pete VanderLaan is on a distinguished road
I have even hxtal'd glass to marble and gone back on the grinders with them joined. Just never pre clean with windex.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #4  
Old 07-17-2019, 09:52 AM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 510
Shawn Everette is on a distinguished road
Yarp, no cleaners with residues. Denatured works, but you should give it a good hand buff after. Xylene's the good stuff, just don't inhale.
Reply With Quote
  #5  
Old 07-17-2019, 12:59 PM
Chris Lowry Chris Lowry is offline
Registered User
 
Join Date: Oct 2003
Posts: 274
Chris Lowry is on a distinguished road
Thanks... I have a piece waiting for itís stainless base but Iíve been scared to try. Iím excited to try the stone idea as well.
Reply With Quote
  #6  
Old 07-17-2019, 02:26 PM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 510
Shawn Everette is on a distinguished road
Hxtal is kind of amazing stuff. It will stick to just about anything, but if the joint has any kind of flex to it, that is where it's likely to fail. They do sell an "amino" prep solution, but I don't know of anyone that actually uses it other than laminaters.
Reply With Quote
  #7  
Old 07-17-2019, 02:57 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,690
Pete VanderLaan is on a distinguished road
I used it back in the '90's but found essentially that 1/2 percent xylene did the same job. Conservation Materials had a pretty good sales rap on the amino stuff and no one ever demonstrated that it was better than snake oil. Pure xylene is not inexpensive and I had a four liter bottle which disturbed me in that it kept evaporating and I could not determine how that could be. I have used the simpler form from Home depot which is cheap but have not been convinced of what other additives might be in it. I do think the xylene gives it tooth. I've seen nothing that I feel contributes to failure in a joint.
For a while, MB was using the pure xylene as a prep and had really bad delam. Once she got right with god and went back to 1/2 % it was fine.

In the optics stuff, it's worth keeping in mind that the glasses being used were annealed to various levels of refinement and some, quite poorly, to the point that shrinkage in the glass itself could contribute to delamination. Do keep in mind that the shrinkage rates between stainless and your host glass can be sufficient enough to cause issues in a thick piece.

I have seen Schott glued to Aluminum and then taken down to about -30F. The joint failed but not at the glue line. The glass cracked about an inch and a half away from that point. Then again, I can't state with real certainty how well that glass was annealed. It's a constant problem that is rarely considered.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #8  
Old 07-17-2019, 04:03 PM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 510
Shawn Everette is on a distinguished road
Quote:
Originally Posted by Pete VanderLaan View Post
Pure xylene is not inexpensive and I had a four liter bottle which disturbed me in that it kept evaporating and I could not determine how that could be.
Sure, "evaporating", that's what all the kids say.

Most of the failure I've seen has been a result of people using a completely inappropriate material, wood, cough, cough. Or their being an issue with one of the components. There is a shelf life for each, and it's impacted by how you store it. I tended to keep the stuff in the fridge, but you had to be patenting about getting it back to room temp. Sometimes as one of them ages, can't remember if it was A or B, it will start to come out of solution. There's a haze that develops, but you can actually bring it back to life with low heat.
Reply With Quote
  #9  
Old 07-17-2019, 04:57 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,690
Pete VanderLaan is on a distinguished road
I am not aware of any shelf life on Hxtal. I continue to use bottles I got ten years back. It's fine. The evaporation was on the xylene.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #10  
Old 07-17-2019, 06:03 PM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 510
Shawn Everette is on a distinguished road
How are you storing it? I would have the stuff turn translucent and lose stability, usually about 18mo. Last time it happened we hit up HIS and they said stick it next to a heat lamp for a day to put back in suspension.
Reply With Quote
  #11  
Old 07-17-2019, 08:00 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,690
Pete VanderLaan is on a distinguished road
I've got it in one gallon containers ( really!) We keep it at around 60F. We do heat it when we are about to mix.
Maybe mine's vintage!
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #12  
Old 07-19-2019, 10:43 PM
Marty Kremer Marty Kremer is offline
Registered User
 
Join Date: May 2004
Location: North Yarmouth ME
Posts: 483
Marty Kremer is on a distinguished road
Quote:
Originally Posted by Chris Lowry View Post
Thanks... I have a piece waiting for itís stainless base but Iíve been scared to try. Iím excited to try the stone idea as well.
I hxtaled glass to aluminum and stored the pieces in a very cold garage over the winter in NY. The aluminum shrunk, the glass didn't, and the hxtal went with the aluminum along with fractures of glass. Had to remake with silicone as the bond.
Reply With Quote
  #13  
Old 07-20-2019, 02:31 AM
Chris Lowry Chris Lowry is offline
Registered User
 
Join Date: Oct 2003
Posts: 274
Chris Lowry is on a distinguished road
Quote:
Originally Posted by Marty Kremer View Post
I hxtaled glass to aluminum and stored the pieces in a very cold garage over the winter in NY. The aluminum shrunk, the glass didn't, and the hxtal went with the aluminum along with fractures of glass. Had to remake with silicone as the bond.
Interesting, so did any of the glue break loose or was there still glass attached to aluminum?
Reply With Quote
  #14  
Old 07-20-2019, 08:07 AM
Marty Kremer Marty Kremer is offline
Registered User
 
Join Date: May 2004
Location: North Yarmouth ME
Posts: 483
Marty Kremer is on a distinguished road
The glue was intact, the glass fractured.
Reply With Quote
  #15  
Old 07-20-2019, 10:35 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,690
Pete VanderLaan is on a distinguished road
I saw exactly the same thing once when John Nickerson hxtal'd Schott to aluminum.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #16  
Old 08-09-2019, 10:57 AM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 510
Shawn Everette is on a distinguished road
Finally needed to mix up some hex and low an behold it was cloudy. Camera work isn't great, but it precipitates as little squareish crystals on the bottom and also on the sides above the liquid line. 12 hours in a hot box and whole thing is crystal clear.
Attached Images
File Type: jpg IMG_20190808_185553478.jpg (19.8 KB, 25 views)
File Type: jpg IMG_20190809_082425775.jpg (34.2 KB, 24 views)
Reply With Quote
  #17  
Old 08-10-2019, 03:12 PM
Greg Vriethoff's Avatar
Greg Vriethoff Greg Vriethoff is offline
rEgisturd Spelunker
 
Join Date: Jan 2007
Location: USSA
Posts: 2,158
Greg Vriethoff is on a distinguished road
Quote:
Originally Posted by Marty Kremer View Post
Had to remake with silicone as the bond.
Have you encountered any problems with this Marty? My understanding is silicone should not be used on aluminum. When it cures it gives off acetic acid which does not play well with aluminum. I've used it once, and the bond has held well for 13 years (still have the piece), but I can see discoloration where the metal joins the glass (clear).
__________________
I loves Dale gilhooly
Reply With Quote
  #18  
Old 08-10-2019, 03:14 PM
Greg Vriethoff's Avatar
Greg Vriethoff Greg Vriethoff is offline
rEgisturd Spelunker
 
Join Date: Jan 2007
Location: USSA
Posts: 2,158
Greg Vriethoff is on a distinguished road
Quote:
Originally Posted by Shawn Everette View Post
Finally needed to mix up some hex and low an behold it was cloudy. Camera work isn't great, but it precipitates as little squareish crystals on the bottom and also on the sides above the liquid line. 12 hours in a hot box and whole thing is crystal clear.
Are you using a vacuum chamber?
__________________
I loves Dale gilhooly
Reply With Quote
  #19  
Old 08-10-2019, 05:52 PM
Marty Kremer Marty Kremer is offline
Registered User
 
Join Date: May 2004
Location: North Yarmouth ME
Posts: 483
Marty Kremer is on a distinguished road
Quote:
Originally Posted by Greg Vriethoff View Post
Have you encountered any problems with this Marty? My understanding is silicone should not be used on aluminum. When it cures it gives off acetic acid which does not play well with aluminum. I've used it once, and the bond has held well for 13 years (still have the piece), but I can see discoloration where the metal joins the glass (clear).
My piece is about that old and I still have it (http://www.kremerglass.com/site2.htm). The glue bond is between the glass and the aluminum billets at the end closest to the ss panel. No discoloration last I looked at about a year ago. The glass- Bullseye Tekta- and the aluminum were sandblasted before glueing.
Reasonable offers will be considered.
Reply With Quote
  #20  
Old 08-12-2019, 10:21 AM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 510
Shawn Everette is on a distinguished road
Not for this batch, bond is hidden. The hot box was just a plastic tub with a lamp in it.
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is Off
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 04:53 AM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2020, Jelsoft Enterprises Ltd.
© CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.