I melted my first batch of Dave's phosphate opal this weekend. It was the straight formula:

(http://talk.craftweb.com/showthread....ight=phosphate)

The compatibility tests did not make it out of the annealer...except for a couple and they blew apart right at the saw. First pic has some all-brossphate pieces to show the color at the top. At the bottom, the broken pieces are inside or outside color-clear...no difference. Last 2 pics show the color intensity achieved for a couple all brossphate pieces.

I've got my work cut out but I'm hoping for a little direction. My only clue is the E&T measurement which for Dave's 2.5% is only 92.6 while Pete's silver opal is 94.1. The silver opal has fit perfectly for me to Cristalica with ring tests for final proof. I have no idea what the Cristalica E&T would be so I have to make a guess that it's closer to Pete's than the Brossphate.

I'd like to intensify the phosphate similar to Jordan's results. Coincidentally, I can raise the E&T to 95.1 by increasing the phosphate 3.6%, but is this really a good way to modify the expansion? Pete usually points to soda ash and sand for moving the expansion. Should I use soda/sand to find a compatible 2.5% glass or just modify the phosphate and see if I can kill 2 birds with 1 stone?

Thanks for any input and to Dave for sharing this formula. My results need work but that was really fun to work with!
Attached Images
File Type: jpg image1 (2).jpg (46.1 KB, 52 views)
File Type: jpg image2.jpg (30.5 KB, 28 views)
File Type: jpg image3.jpg (25.9 KB, 32 views)
Reply With Quote
  #2  
Old 05-01-2018, 07:41 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 22,085
Pete VanderLaan is on a distinguished road
cristalica is currently about a 97.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #3  
Old 05-01-2018, 12:57 PM
Dan Vanantwerp
Guest
 
Posts: n/a
OK...that gives me a direction. Thanks.
Reply With Quote
  #4  
Old 05-01-2018, 03:25 PM
Jordan Kube Jordan Kube is offline
?
 
Join Date: Aug 2003
Location: Seattle, WA
Posts: 1,704
Jordan Kube is on a distinguished road
Using Dave's calculator I would shoot for 91 LEC for something compatible with Cristalica. My notes indicate the more phosphate you add the lower your target number will be. I melted a 5% that showed 1 point high in a trident seal but no stress showed in the product under the polarimeter. The calculator shows a theoretical 87.75 LEC. Melting a phosphate opal will yield different results than a straight soda lime calcedonia. You can really only rely on your previous phosphate tests as a guide.
__________________
WWUD? Think for yourself.
Reply With Quote
  #5  
Old 05-01-2018, 04:29 PM
Dan Vanantwerp
Guest
 
Posts: n/a
Wow...thanks Jordan! I had a hunch that making LEC adjustments with the phosphate was a bad idea. I am awaiting a package of a la carte ingredients from Jim at East Bay including his sand. I'll be able to tune this in a bit on my next batch.

I'd be interested to know if you got the fit worked out for the 5% with 1/2 borax and if it needs 2300 to melt.
Reply With Quote
  #6  
Old 05-01-2018, 05:11 PM
Jordan Kube Jordan Kube is offline
?
 
Join Date: Aug 2003
Location: Seattle, WA
Posts: 1,704
Jordan Kube is on a distinguished road
I considered the 5% recipe compatible due to the product showing no stress. I melted at 2300 and I would recommend higher if possible. Go ahead and make LEC adjustments, just don't rely on your non phosphate batches as a guide.
__________________
WWUD? Think for yourself.
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 03:48 PM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2020, Jelsoft Enterprises Ltd.
CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.