Tellurium

Does anyone know what color Tellurium imparts to glass? This is a payback for help on sodium silicate ."Tellurium is also used to color glass and ceramics and is one of the primary ingredients in blasting caps". Ron
Reply With Quote
  #2  
Old 08-24-2017, 06:45 PM
Ron Mynatt Ron Mynatt is offline
Registered User
 
Join Date: Apr 2008
Location: Springdale Arkansas
Posts: 128
Ron Mynatt is on a distinguished road
I checked Coloured Glasses by W.A.Weyl and he had a section on it so I think I have an answer that I can pass on.
Reply With Quote
  #3  
Old 08-27-2017, 09:03 PM
Dave Bross Dave Bross is offline
Registered User
 
Join Date: Apr 2002
Location: Archer FL(near Gainesville)
Posts: 2,903
Dave Bross is on a distinguished road
Paraphrasing Volf from Chemical approach:

Heavy reduction or it volatilizes.

Coral red under heavy reduction, steel grey if annealed slowly.

Pink to purple-red i phosphate glasses on cooling.
__________________
Art is not a thing...it's a way.
Reply With Quote
  #4  
Old 09-22-2017, 11:47 AM
Bradley Howes Bradley Howes is offline
Registered User
 
Join Date: Mar 2015
Location: Palo Alto, CA
Posts: 35
Bradley Howes is on a distinguished road
Looking at Weyl's book, though he and Smiley were able to produce a purple glass (Glass Science Bull., 1947, 6, 38.), he doesn't consider it "practical'. Under oxidizing conditions, a sodium-barium-aluminum phosphate glass with 1% metallic Tellurium produced the purple glass. He also says it can be considered an analogue of selenium pink, which I believe is colloidal.
__________________
I have to be the best at what I do. If I didn't succeed the first time then I didn't try hard enough. This is to say I expect myself to do the best I can. Don't get me wrong, mistakes are great for learning.
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is Off
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 03:26 AM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2018, Jelsoft Enterprises Ltd.
CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.