My gf is making a cast piece roughly 6"(w)X 4.5"(h)x7.75"(l). According to Bullseye thick slab annealing tips, "... or is anything besides a flat slab of uniform thickness, select an annealing cycle for a piece that is twice the thickness of the thickest area of the piece."

So based on this they recommend app. 1300 hrs! to room temperature with anneal at 900 for about 64 hours then the rest cool down.

We had based it on 1/8" per hour for anneal to get to midpoint of the h. and came up with about 20 hours anneal but then we are at kind of a loss for the rest of the cool down.

any ideas would be appreciated,

fredi
Reply With Quote
  #2  
Old 05-05-2019, 12:29 PM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 328
Shawn Everette is on a distinguished road
Quote:
Originally Posted by Fredi Vilina View Post
select an annealing cycle for a piece that is twice the thickness of the thickest area of the piece."fredi
I don't know that I've ever gone that route. 20 hours may be a bit shy, closer to 24-30, but you're not casting the lens for for the Hubble. As a general rule I go 1.5-2 times longer than my annealing cycle through strain, about 200 less than anneal. I then double that time down to room temp. For example 24hr @900, 60hr to 700, 120hr to 150.

Things like appendages will have me opt for longer cycles, but I've used this method without fail.
Reply With Quote
  #3  
Old 05-05-2019, 01:08 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,334
Pete VanderLaan is on a distinguished road
Keep it off the floor.

Try to obtain a copy of "The schedules" by Graham Stone.

Based in my experience, I don't think of Shawn's soak to be long enough. I'd double it. Keep in mind that once you pass the strain point, no further annealing can occur. You're simply trying to prevent thermal shock.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #4  
Old 05-05-2019, 05:21 PM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 328
Shawn Everette is on a distinguished road
That was more to keep an example of how to calculate, I'd probably use that for something in the 5" range. Bullseye is calling for 32hrs for 8", which I might use, but though strain is 370hrs. I've never annealed for 16+ days.
Reply With Quote
  #5  
Old 05-05-2019, 06:04 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 21,334
Pete VanderLaan is on a distinguished road
I'm considering oversized paperweights I've seen on and off and the sucessful soak cycles were really long... really really long. Graham identifies them and lays them out. If you don't have the book, it's one of the mayflies out there.

In a piece of this scale, which isn't all that big. I'd make a clear one first and when done with a long cycle, I'd look in the tell tail tool, the polariscope. Witness pieces are incredibly helpful at simply documenting the event. I know the Simpson planets were in for several months. We never did a clear one though.
Keeping it cooling evenly is important. Keep it off the floor and multiple thermocouples, all over the place are simply smart. Eventually the cost of electricity cooling far out weighs the cost of casting.

I have some castings here that took sixteen years to crack.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #6  
Old 05-06-2019, 09:15 AM
Shawn Everette Shawn Everette is offline
Registered User
 
Join Date: Mar 2013
Location: Indianapolis, IN
Posts: 328
Shawn Everette is on a distinguished road
The 12" paperweight we made at Penland annealed for maybe a week, and we rolled it down the hill. Chipped from our shenanigans, but no real fractures. Glass is s funny thing sometimes.
Reply With Quote
  #7  
Old 05-06-2019, 02:43 PM
Fredi Vilina Fredi Vilina is offline
Registered User
 
Join Date: Jun 2002
Location: St. Paul MN
Posts: 245
Fredi Vilina is on a distinguished road
thanks

As usual, always helpful and slightly amusing! we have a time crunch of 7 days so we are going to try it with that for the kiln casting. we also have the same one made for ladle casting and we'll anneal that one really long. They will both be clear so I'll let you know what the end results are. the difference though, is the kiln cast is old blenko and the ladle casting will be spruce.
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is Off
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 04:58 PM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2019, Jelsoft Enterprises Ltd.
CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.