Casting a new crown.

I'm looking for some advice. I am building a new furnace and looking at my old crown I see that the skin it is peeling in layers.
Are used to cast a light 30. Are there any recommendations for a crown that would last longer without peeling?
Reply With Quote
  #2  
Old 07-12-2017, 02:18 PM
Eben Horton Eben Horton is online now
Registered User
 
Join Date: Apr 2002
Location: Wakefield, RI
Posts: 4,159
Eben Horton is on a distinguished road
Can't beat castolite 30 imho..... crowns are meant to be replaced every 10-15 years I think.

That said, a friend used huge silicon carbide kiln shelves as a crown and swears by them.
Reply With Quote
  #3  
Old 07-12-2017, 04:15 PM
Kenny Pieper Kenny Pieper is offline
Registered User
 
Join Date: Feb 2003
Location: Burnsville N.C.
Posts: 796
Kenny Pieper is on a distinguished road
Quote:
Originally Posted by Mike Kaplan View Post
I'm looking for some advice. I am building a new furnace and looking at my old crown I see that the skin it is peeling in layers.
Are used to cast a light 30. Are there any recommendations for a crown that would last longer without peeling?
If you are melting batch I would recommend that you use something harder and more durable than cast a lite 30. Ask your refractory source. There are so many options now days.
Reply With Quote
  #4  
Old 07-12-2017, 10:42 PM
Mike Kaplan Mike Kaplan is offline
Registered User
 
Join Date: Apr 2002
Location: cleveland ohio
Posts: 208
Mike Kaplan is on a distinguished road
Thx for the advice. I always seem to forget to ask the experts first.
Reply With Quote
  #5  
Old 07-13-2017, 08:57 AM
Mike Kaplan Mike Kaplan is offline
Registered User
 
Join Date: Apr 2002
Location: cleveland ohio
Posts: 208
Mike Kaplan is on a distinguished road
I would say this crown lasted 3 yrs and i use cullet. It didnt crack but it is pealing
Reply With Quote
  #6  
Old 07-13-2017, 10:35 AM
Justin Zotynia Justin Zotynia is offline
Registered User
 
Join Date: Aug 2009
Location: Bushkill, PA
Posts: 56
Justin Zotynia is on a distinguished road
I used kastolite 30 for my crown and used cullet worked well no peeling. maybe every furnace environment is different due to design. don't know just that it worked for me.
Reply With Quote
  #7  
Old 07-13-2017, 10:40 AM
Jordan Kube Jordan Kube is online now
?
 
Join Date: Aug 2003
Location: Seattle, WA
Posts: 1,570
Jordan Kube is on a distinguished road
I would use something a little heavier duty than Kast-o-lite. Some people have good success with it. It doesn't seem to be the case in your furnace. Make sure you mix thoroughly and to manufacturer's instructions as well.
__________________
WWUD? Think for yourself.
Reply With Quote
  #8  
Old 07-13-2017, 11:44 AM
Eben Horton Eben Horton is online now
Registered User
 
Join Date: Apr 2002
Location: Wakefield, RI
Posts: 4,159
Eben Horton is on a distinguished road
I'd bet you a case of beer that when you made your crown 3 or 4 years ago, you made th mix too wet. If you mix it right, it will last a long long time. Mix it wet and the casting will be brittle and won't last. I learned this with glory hole and furnace doors. Also, make it thick. At least 4 inches and give it a nice arch to give it strength
Reply With Quote
  #9  
Old 07-13-2017, 11:44 AM
Eben Horton Eben Horton is online now
Registered User
 
Join Date: Apr 2002
Location: Wakefield, RI
Posts: 4,159
Eben Horton is on a distinguished road
Oh.... I forgot to mention, I would use castolite 30 plus. Not the stock castolite 30
Reply With Quote
  #10  
Old 07-13-2017, 12:21 PM
Sky Campbell's Avatar
Sky Campbell Sky Campbell is offline
Registered User
 
Join Date: May 2002
Location: Gainesville FL
Posts: 836
Sky Campbell is on a distinguished road
Quote:
Originally Posted by Eben Horton View Post
I'd bet you a case of beer that when you made your crown 3 or 4 years ago, you made th mix too wet. If you mix it right, it will last a long long time. Mix it wet and the casting will be brittle and won't last. I learned this with glory hole and furnace doors. Also, make it thick. At least 4 inches and give it a nice arch to give it strength
That has been my experience. To much water and it spalls over time. Don't forget to vibrate air voids are weak points.
I really can't imagine a better product for a crown. I have never found a product that compares. Green cast for an early furnace failed miserably.

Last edited by Sky Campbell; 07-13-2017 at 12:23 PM.
Reply With Quote
  #11  
Old 07-13-2017, 07:26 PM
Art Freas Art Freas is online now
Registered User
 
Join Date: Aug 2014
Location: Washington
Posts: 452
Art Freas is on a distinguished road
OK, I am almost ready to post my door learnings but want one more round before I do it. However one thing I would say for doors. If it vibrates down it is probably too wet. If you put 9 pints with 55lbs you can tamp it but not really vibrate it. So far extremely dry and tamped is working pretty well. Not sure how that would work with a dome form though.
Reply With Quote
  #12  
Old 07-13-2017, 08:50 PM
Eben Horton Eben Horton is online now
Registered User
 
Join Date: Apr 2002
Location: Wakefield, RI
Posts: 4,159
Eben Horton is on a distinguished road
Quote:
Originally Posted by Art Freas View Post
OK, I am almost ready to post my door learnings but want one more round before I do it. However one thing I would say for doors. If it vibrates down it is probably too wet. If you put 9 pints with 55lbs you can tamp it but not really vibrate it. So far extremely dry and tamped is working pretty well. Not sure how that would work with a dome form though.
Spot on. I mix mine so dry you'd think it's way too dry but it hardens rock solid. When I fill forms to cast parts, I add small amounts at a time and trowel it down and compress it into corners to assure there are no voids. That said I have never tried the vibration technique
Reply With Quote
  #13  
Old 07-15-2017, 08:08 PM
Peter Bowles Peter Bowles is offline
Registered User
 
Join Date: Sep 2002
Location: Breadalbane, Tasmania
Posts: 609
Peter Bowles is on a distinguished road
I would urge you to find a way to vibrate the castable as it goes into the mold - it will make a significant difference to the final density of the casting.
It does mean you have to have the mold very securely braced and any gaps filled, but you will get a much better result than by just tamping alone. It also means you can use the specified quantity of water too - which as already mentioned is a critical aspect of these materials.
There are many inexpensive pneumatic vibrators available now - a seriously worthwhile investment I think. I used to set molds up on an old reciprolap with great success, but now use a wee hand held thing.
Once you see these castables flow under vibration you'll understand how tamping just won't cut it - particularly for structural castings.
Reply With Quote
  #14  
Old 07-15-2017, 08:24 PM
Peter Bowles Peter Bowles is offline
Registered User
 
Join Date: Sep 2002
Location: Breadalbane, Tasmania
Posts: 609
Peter Bowles is on a distinguished road
If your molds are reusable, permanently mark on them the final volume or weight of the castable used. Will make the whole process much more economical in time and materials next time around.
Reply With Quote
  #15  
Old 07-15-2017, 11:12 PM
Steve Stadelman Steve Stadelman is offline
Registered User
 
Join Date: Jun 2002
Location: Portland oregon area
Posts: 3,728
Steve Stadelman is on a distinguished road
Peter is right on with sage advice. Harbor Freight makes a pin vibrator that's practically disposable for just these occasions.
__________________
If all you wanted to do was express yourself artistically, you should have obtained a field watercolor set and a pad of acid-free paper. You chose a media with INFRASTRUCTURE baby!
Reply With Quote
  #16  
Old 07-16-2017, 01:57 AM
Dennis Hetland Dennis Hetland is offline
Registered User
 
Join Date: Sep 2009
Location: Salem, OR
Posts: 304
Dennis Hetland is an unknown quantity at this point
Is this a combustion furnace? I Don't understand why you would run a combustion furnace for cullet.
It's not one of those electric furnaces the have u shaped elements dropping through the roof is it? Those furnaces have holes in the roof where your money flies out.
IF It's an electric furnace and you're melting cullet I wouldn't use castable. It has very poor insulating properties compared to IFB.
__________________
candlewoodglass@gmail.com
Reply With Quote
  #17  
Old 07-16-2017, 07:56 AM
Michael Ahlefeldt-Laurvig Michael Ahlefeldt-Laurvig is online now
Registered User
 
Join Date: Apr 2010
Location: Sweden
Posts: 643
Michael Ahlefeldt-Laurvig is on a distinguished road
In my oil fired 350 kg pot furnace I got talked into using the lite 30 by a salesman- in spite of having had a crown like that fail on me before- After 2 years it failed and I replaced it with Greencast 94- after 15 years when that furnace was retired the crown looked like it was new.
Dennis , in my case the choice of combustion furnace was due to the power company- I needed 100 amp 400 volt 3 phase main fuses. My studio was a couple of miles from the transformer they would have to upgrade from. out in the country.The cost proposal almost 30 years ago was 30,000 just to do it + change a local transformer 7000, then the labor and cost of 300 meters cable to my studio- that money would have bought a small farm at the time.
Also, dense cast crowns are usually insulated on the outside :-)
Reply With Quote
  #18  
Old 07-16-2017, 08:58 AM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 19,813
Pete VanderLaan is on a distinguished road
I would not be inclined to make the hot face of a crown with insulating castable. I would make it out of a high alumina castable and make damn sure that I didn't have to remove the crown to change the pot. Cheyenne is making his moly's that way now. The vibrator is critical to a good casting, particularly if it's five inches thick.
The single best high alumina castable I've ever used is MORCO 95 ( Missouri Refractory Company). High Temp in Fenton Missouri handles it and accept no substitutes. I had a crown in service for five years with it and it looked brand new. I would insulate the snot out of it with both 2600F and standard 8lb density fiber. Then I would go to enormous lengths to never touch it again.

As to cullet, it can be very deceptive stuff. The borax that keeps winding up in those products has a poor ionic bond and dissociates pretty easily. Boron is really good at attacking both silicates and fireclays. It's that yellow fluff near your door that is dissolving everything. There's no free lunch. If your cullet melts easily at low temperatures, there's a reason. Put a vent on your electric units if you do use cullet. Just plug the vent when you aren't melting.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #19  
Old 07-16-2017, 11:06 AM
Dennis Hetland Dennis Hetland is offline
Registered User
 
Join Date: Sep 2009
Location: Salem, OR
Posts: 304
Dennis Hetland is an unknown quantity at this point
I designed front loading electric furnaces. The front tears away in two stages. You can just disassemble the archway, but you can disassemble the bottom as well to get inside for maintenance. It's all machined IFB. No walls to demolish and recast. You can simply replace single bricks. (that you can buy from me for only $10)
I've met Cheyenne a couple of times. He's a friend of a friend and makes a good product. I don't have anything against Cheyenne, but my furnaces are much more efficient. I have 27" of insulation on top of the crown with no penetrations. Plus my design creates firing chamber that is 25% smaller than a molly furnace.
__________________
candlewoodglass@gmail.com
Reply With Quote
  #20  
Old 07-16-2017, 11:45 AM
Eric Trulson Eric Trulson is offline
Young Turk
 
Join Date: Sep 2014
Location: NH
Posts: 70
Eric Trulson is on a distinguished road
Quote:
Originally Posted by Peter Bowles View Post
I would urge you to find a way to vibrate the castable as it goes into the mold - it will make a significant difference to the final density of the casting...Once you see these castables flow under vibration you'll understand how tamping just won't cut it - particularly for structural castings.
One more voice in the chorus of agreement here. Vibrating is 100% necessary for castables that are intended for it (it will usually say in the manufacturer's datasheet whether a castable is intended to be vibrated or rammed).

There are good cheap commercial vibrators available, but in a pinch I've used a sawzall with the blade taken out, just pressing it up hard against the side of the mold and holding down the trigger, and giving the mold a little shimmy back and forth by hand at the same time. You will be able to see when the vibration "takes", the castable starts to flow much more quickly and gets a very faint liquid sheen on the surface (NOT water pooling up on the top of the castable. That generally means you have over-vibrated and it's time to stop)
Reply With Quote
  #21  
Old 07-17-2017, 12:40 AM
David Hopman David Hopman is offline
Registered User
 
Join Date: Mar 2009
Location: Sutter Creek, CA
Posts: 413
David Hopman is on a distinguished road
The cheap air hammer I bought to chisel through glass buildup on the furnace also worked great as a vibrator for the castable.
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is Off
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 03:18 PM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2018, Jelsoft Enterprises Ltd.
CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.