Looking for some advice from the experts. I have mostly just batched from recipes from Petes colour class. I am looking to batch a manganese purple. Trying to replace soda with more potash, and eliminate lithium and borax. Here's what I thought I might start with, given what I have on hand.
Silica 83lbs
Potash 30 lbs
Soda Ash 6.5 lbs
Feldspar 8 lbs
Barium Carb. 3.5lbs
Zinc Oxide 1 lbs
Pot. Nitrate .25lbs
Antimony Oxide .25lbs

E and T 94.6

Initially this would be used as a stand alone batch. Hopefully as a base where the colour intensity could be varied easily by increasing or decreasing manganese
Reply With Quote
  #2  
Old 02-24-2023, 02:58 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 24,477
Pete VanderLaan is on a distinguished road
just remember, no antimony in the purple. It makes it harder to fine out but.. tough.
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #3  
Old 02-27-2023, 07:07 PM
Josh Bernbaum Josh Bernbaum is offline
Registered User
 
Join Date: Feb 2009
Location: Brattleboro, VT
Posts: 957
Josh Bernbaum is on a distinguished road
If you're making color bars or casing this with clear, I'd agree it'd probably be helpful to have that much potash vs. soda ash in there, but if you plan on just making things (especially thin things) out of this current ratio of alkali I'd think it'll be too "fat" of a glass to work with any ease. I've gotten some really nice vibrant purple from manganese with about half and half potassium and sodium. I like an ooch of cobalt in there too.
__________________
www.jmbglass.com
instagram.com/joshbernbaum_glass
Reply With Quote
  #4  
Old 02-28-2023, 11:05 AM
Greg Vriethoff's Avatar
Greg Vriethoff Greg Vriethoff is offline
Drone
 
Join Date: Jan 2007
Location: Charlotte, NC
Posts: 2,390
Greg Vriethoff is on a distinguished road
Now I have to ask.

What's an "ooch"?
__________________
Temperature and time.
Reply With Quote
  #5  
Old 02-28-2023, 12:30 PM
Pete VanderLaan's Avatar
Pete VanderLaan Pete VanderLaan is offline
The Old Gaffer
 
Join Date: Apr 2002
Location: Chocorua New Hampshire
Posts: 24,477
Pete VanderLaan is on a distinguished road
A pooch that's been screwed?
__________________
Where are we going and why am I in this basket?
Reply With Quote
  #6  
Old 03-02-2023, 04:23 PM
Mark Armstrong Mark Armstrong is offline
Registered User
 
Join Date: Nov 2009
Location: Wellington, Ontario, Canada
Posts: 70
Mark Armstrong is on a distinguished road
Thanks for that Josh, I will start with a half and half soda/potash.
I have been looking at the Helmer recipes to get a ball park on the manganese/cobalt proportions. It won't be for 2 or 3 weeks, but i will probably do a 35lb melt. I'll report back
Reply With Quote
Reply


Thread Tools
Display Modes

Posting Rules
You may not post new threads
You may not post replies
You may not post attachments
You may not edit your posts

BB code is On
Smilies are On
[IMG] code is On
HTML code is Off
Forum Jump


All times are GMT -5. The time now is 10:16 PM.


All published comments within these message boards are the opinions of its contributor and does not represent
the opinion(s) of the owner(s) of this website. Please see the Terms of Use file for more details.

Books to Help Artists Avoid Online Scams: Top 10 Email Scams | Social Media Scams

Powered by vBulletin® Version 3.7.2
Copyright ©2000 - 2023, Jelsoft Enterprises Ltd.
CraftWEB.com. Opportunity Network. 2008. All Rights Reserved.